Regulation 446. Cold bend tests

Official text — not yet verifiedGazette 1 Oct 2026 · printed pp. 770–771Figure referenced

Not yet checked against the official Gazette; verify before relying on it.

Reproduced from the Gazette of India · verification status above

446.Cold bend tests.─ (1) Two bend tests shall be made as given in this regulation.

(2)One specimen shall be tested with outer surface of the weld in tension, and the other with the inner surface in tension. The specimens shall be rectangular in section and shall be cut out transversely to the weld so as to have a width not less than one-and-a-half times the thickness of the plate. The sharp corners of the specimens shall be rounded to a radius not exceeding 10 percent of the thickness of the specimen.

(3)The specimen to be tested with the outer surface of the weld in tension shall be prepared by cutting to waste the metal local to the inner surface of the weld, so that the desired specimen thickness is obtained (see A, Figure 12/78). The specimen to be tested with inner surface in tension shall be prepared by cutting to waste the metal local to the outer surface of the weld so that the desired specimen thickness is obtained (see B, Figure 12/78). Where the thickness of the plate permits, both specimens may be cut from the same piece of plate, the specimens being located in the plate one above the other (See C, Figure 12/78).

(4)Each specimen shall be mounted with the weld midway between the supports set apart at a distance of not more than 5.2 times the thickness of the specimen and pushed through the supports with a former having a diameter equal to three times the thickness of the specimen.

(5)On completion of the test, no crack or defect at the outer surface of the specimen shall be greater than 1.6 mm measured across the specimen, or 3 mm measured along the length of the specimen. Premature failure at corners of the specimen shall not be considered cause for rejection.

Figures cited in this regulation (1, exact crops of the Gazette)

Gazette Fig. 12/78
Fig. 12/78(no caption printed with this figure)
View Gazette page 819 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Independent explanation — not the law · draft · engineer review in progress

In short

Sets the two cold bend tests (outer surface and inner surface in tension) for Class II boiler test plates.

Key points

  • (2) One specimen has the outer weld surface in tension and the other the inner surface. Specimens are rectangular, cut across the weld, at least one-and-a-half times the plate thickness wide, with corners rounded to no more than 10 percent of specimen thickness.
  • (3) Each specimen is made by cutting away metal on the opposite side of the weld (A and B, Figure 12/78). Both may come from the same piece of plate, one above the other, if thick enough (C).
  • (4) The weld sits midway between supports no more than 5.2 times the specimen thickness apart, and is pushed through with a former of diameter three times the specimen thickness.
  • (5) After the test, no crack or defect at the outer surface may exceed 1.6 mm across the specimen or 3 mm along its length.

Watch out

  • The crack limit across the specimen here is 1.6 mm, which differs from the Class I limit in regulation 438.
  • Premature failure at the specimen corners is not a cause for rejection.

Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.

Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).

Orientation hints (unverified)

These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.

Historical 1950-edition reg.Heading as OCR'dHeading similaritySource image
19Bend Tests100%Chapter II (DPIIT scan), image 2
84Bend Tests100%Chapter II (DPIIT scan), image 16
262Bend Tests100%Chapter V (DPIIT scan), image 7

Amendment history of the candidate IBR 1950 regulations: Reg. 19 (1 amendment)

IBR 1950 regulation 19 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 19 page for its amendments.

Reg. 19
MATERIALS OF CONSTRUCTION

STEEL PLATES, RIVETS, SECTION AND BARS IN CARBON STEEL

Bend Tests

Cold Bends.-(a) Test pieces shall be sheared lengthwise or crosswise from plates or bars, and shall not be less than 1½ inches wide, but for small bars the whole section may be used. For rivet bars bend tests are not required.

b) In all cold bend tests, on samples 0.5 inch in thickness and above, the rough edge or arris caused by shearing may be removed by filing or grinding, and samples 1 inch in thickness and above may have the edges machined, but the test pieces shall receive no other preparation. The test pieces shall not be annealed unless the material from which they are cut is similarly annealed in which case the test piece shall be similarly and simultaneously treated with the material before testing. 

(c) (i) For bend test of plates of all grades of steel, the test piece shall withstands, without fracture, being bent cold through 180o around a mandrel, the radius of which shall have a relationship to the plate thickness as given below:

      Tensile strength                          Mandrel Radius

      36 - 49 kg./mm2                              1 T

      41 - 57 kg./mm2                              1 T

      45 - 64 kg./mm2                            1.5 T

where T = Plate thickness  

(ii) For cold bend test of sections and bars, the test piece shall withstand, without fracture, being doubled over until the internal radius is equal to that shown in Table under regulation 16 and the limbs are parallel.

(d) For small sectional material these bend tests may be made from the flattened bar.

(e) Bend tests may be made either by pressure or by blows.

IBR 1950 regulation 84 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 84 page for its amendments.

Reg. 84
MATERIALS OF CONSTRUCTION

FORGED OR ROLLED PRESSURE PARTS OTHER THAN SEAMLESS DRUMS OF CARBON STEEL

Bend Tests

(a) Bend test pieces shall be of rectangular cross section machined to a finished size of 1 inch wide by ¾ inch thick. In the case of headers, bend test pieces may be cut transversely 1½ T wide by T thick where T is the thickness of the header. The edges shall be rounded to a radius of 1/16 inch. The test pieces shall be bent over the thinner section.

(b) Test pieces shall be bent when cold through an angle of 180° without fracture, the internal radius of the bend being not greater than that specified in table below for the 1 inch wide by ¾ inch thick test piece and not more than 1½ T for the full thickness test piece:

Ultimate tensile stress

Internal radius of bend

Tons/sq. inch

Inch

Upto 32 1/4
Above 32 and upto 36 3/8
Above 36 and upto 38 5/8

Bend tests may be made by pressure or by blows.
IBR 1950 regulation 262 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 262 page for its amendments.


Reg. 261
, Reg. 262, Reg. 263

Bend Test Pieces

a)

One for direct and one for reverse bending shall be taken transversely to the weld and where the thickness of the plate permits, one should be above the other. The specimens shall be rectangular in section so as to have width equal to one and half times the thickness of the specimen but not less than 30 mm. The surface of the specimens shall be machined just to remove the surface irregularities of the plate and the weld. The corners of the specimens shall be rounded to a radius not exceeding 10% of the thickness of the specimen.
b)

Where plate thicknesses do not exceed, 1¼ in. the thickness of the specimen shall be equal to the full thickness of the test plate. Where the plate thickness exceeds 1¼ in. the specimen shall in all cases have a thickness of at least 1¼ in. The specimen to be tested with the outer surface of the weld in tension shall be prepared by cutting to waste the metal local to the inner surface of the weld so that the desired specimen thickness is obtained (see Fig.20, Specimen A). the specimen to be tested with the inner surface in tension shall be prepared by cutting to waste the metal local to the outer surface of the weld so that the desired specimen thickness is obtained (see Fig.20, Specimen B). Where the thickness of the plate permits, both specimens may be cut from the same piece of plate, the specimen being located in the plate one above the other (see Fig. 20, Specimen C).



Reg. 262

Bend Tests

The specimen shall be mounted in such a way that the axis of the former is in the middle of the weld, and on roller supports the faces of which are separated by a distance determined by the thickness of the specimen.

The test specimen shall be pushed through the supports by a former having a diameter also determined by the thickness of the specimen. The requirements of the Table below, relating to the thickness of the test specimen shall apply.

 Table: Bend Test Requirements

Specified minimum tensile strength of plate Diameter
of former
Free space between supports at the end of test
Below 44 kgf/mm² 2t 4.2t
From 44 to 54 kgf/mm² 3t 5.2t
Above 54 kgf/mm² 4t 6.2t

On completion of the test, no crack or defect on the outer surface of the specimen shall be greater than 1.5 mm measured across the specimen, or 3 mm measured along the specimen. Premature failure at the corner of the specimen shall not be considered as a cause for rejection.



Reg. 263

Notched-Bar Impact Tests

The notched bar impact test specimens are to be one of the two types and dimension shown in figure 21A and 21B. The notch shall be contained in the weld-metal at approximately the axis of the weld and the axis of the notch is to be perpendicular to the surface of the plate.

The test shall be carried out as follows:-
For the U-Notch specimen at a temperature of 20 ± 2°C.
For the V-Notch specimen at a temperature of 50 ± 2°C.
In the case of V-Notch specimen, the machining of the bottom of the notch shall be done very carefully.

The choice between U-notch and V-notch specimen shall be at the discretion of the Inspecting Authority. The minimum result to be obtained from the Impact test pieces shall be:

a) U-notch specimen 5.50 kgfm/cm²
b) V-notch specimen 3.46 kgfm/cm²

Note: Above values are equivalent to 2.76 kgfm divided by sectional area below the notch.

Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Instrument
Indian Boiler Regulations, 2026 (made by the Central Boilers Board under s.40 of the Boilers Act, 2025)
Notification
F.No. P-30014/3/2021-Boiler dated 7 Aug 2026
Published
Gazette of India, Extraordinary, Part III Sec. 4, No. 596, 1 Oct 2026 (CG-DL-E-06102026-276813)
In force
1 Oct 2026 (reg. 1(3): date of publication in the Official Gazette)
Printed Gazette page
770–771
PDF page index
770–771 · open official e-Gazette PDF
Extraction
pdftotext layout mode, sequential regulation detector · text hash 6ee6a4a08b38a0b0
Verification
Official text — not yet verified
Amendments checked
None known after 1 Oct 2026 as of build date (not a guarantee). Amendment log
How to cite

Indian Boiler Regulations, 2026, reg. 446, Regulation 446, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.770–771. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).

The citation refers to the government publication. Cite the Gazette, not this website.

Help improve this page