Indian Boiler Regulations, 2026 · Chapter 3 · Construction and Workmanship
Regulation 97. Fusion butt welded longitudinal seams
Not yet checked against the official Gazette; verify before relying on it.
97. Fusion butt welded longitudinal seams.─ Where the longitudinal seam is fusion butt welded, the precautions shall be observed as follows:
(i)Plates 20 mm and above in thickness shall be bevelled from both sides of each abutting edge but the bevel need not necessarily be the same on each side (see Figs. 3/1 and 3/2). Plates less than 20 mm in thickness may be bevelled from one side only of each abutting edge (see Figs. 3/3 and 3/4).The included angle of the bevel shall be not less than 60o and the bevelling may be any one of the forms shown in Figs. 3/1 to3/4.
Fig. 3/1 Fig.3/2 Fig. 3/3 Fig. 3/4
(ii)In order to obtain full penetration of the weld metal, a gap shall be maintained between the plates when they are being welded. Joints shall be welded from both sides, and the slag shall be removed after making each run. Before the second side of the joint is welded any slag or defect at the bottom of the first run shall be removed by grinding, chipping or machining. There shall be no appreciable undercutting of the plate.
(iii)For the purposes of relieving internal stresses, the plates adjacent to a fusion weld shall be efficiently annealed after welding.
Figures cited in this regulation (4, exact crops of the Gazette)

View Gazette page 565 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)

View Gazette page 565 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)

View Gazette page 565 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)

View Gazette page 565 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
In short
Regulation 97 lists the precautions for fusion butt welded longitudinal seams: edge bevelling, full penetration and annealing.
Key points
- (i) Plates 20 mm and thicker are bevelled from both sides (Figs. 3/1 and 3/2). Thinner plates may be bevelled from one side (Figs. 3/3 and 3/4). The included angle is at least 60°.
- (ii) A gap is kept between plates for full penetration. Joints are welded from both sides and slag is removed after each run. Before welding the second side, slag or defects at the root of the first run are removed by grinding, chipping or machining. There must be no appreciable undercutting.
- (iii) Plates next to the weld are efficiently annealed after welding to relieve internal stresses.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
| Historical 1950-edition reg. | Heading as OCR'd | Heading similarity | Source image |
|---|---|---|---|
| 108 | Longitudinal Seams | 100% | Chapter III (DPIIT scan), image 1 |
IBR 1950 regulation 108 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 108 page for its amendments.
| Reg. 108, Reg. 109, Reg. 110 SHELLS, ANGLE RINGS, BUTT STRAPS, ETC. Longitudinal Seams |
| The longitudinal seams of shell belts shall be butt-jointed with double straps when the diameter or Working Pressure exceeds the limits stated below :-
Butt straps shall be cut from the shell plates, or, alternatively, all the butt straps of each required thickness shall be cut from one plate. The lengths of the straps wherever practicable shall be transverse to the direction of rolling of the plate. Straps shall be pressed or bent in rolls to the shell curvature. Reg. 110 SHELLS, ANGLE RINGS, BUTT STRAPS, ETC. Thinning of Butt Straps |
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Indian Boiler Regulations, 2026, reg. 97, Regulation 97, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.565. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.