Regulation 123. Requirements of Post Weld Heat Treatment(PWHT)

Official text — not yet verifiedGazette 1 Oct 2026 · printed pp. 573–579TableFigure referencedFormula / symbolsLong provision

Not yet checked against the official Gazette; verify before relying on it.

Reproduced from the Gazette of India · verification status above

123. Requirements of Post Weld Heat Treatment(PWHT).─ The requirements of Post Weld Heat Treatment(PBWH) shall be as provided in Table 3/5

Serial No.Material group (as per Table 2/1)PWHTPWHT not required under the following conditions:
(1)(2)(3)(4)
1M1 Group 1, M1 Group 2595°C min(i) For All Product Forms:
(a) nominal weld thickness (t) ≤ 20 mm; and
(b) If preheated to 95°C min when nominal
weld thickness (t) ≤ 20 mm and nominal base
metal thickness ≤ 25 mm; and
(c) C ≤ 0.25%;
(ii) Only for tubes and pipes, if 0.25% < C ≤
0.3% and nominal thickness ≤ 9 mm; In case
of welded stays, diameter of stay is not used to
determine preheat requirements.
2M3 Group 1595°C min(a) For all product forms nominal wall
thickness (t) ≤ 16 mm except for tubes and
pipes t ≤ 13 mm & OD ≤ 127 mm; and
(b) C ≤ 0.25%
3M4 Group 1650°C min(a) For all product forms nominal base metal
thickness t ≤ 16 except for tubes and pipes
t ≤ 13 mm & OD ≤ 127 mm; and
(b) C ≤ 0.15%; and
(c) Preheat 120°C min
4M5A Group 1 &
M5B Group 1
675°C min(a) For all product forms nominal base metal
thickness t ≤ 16 except for tubes t ≤ 13 mm &
OD ≤ 127 mm and for pipes t ≤ 13 mm & OD
≤ 127 mm; and
(b) Cr ≤ 3%; and
(c) C ≤ 0.15%; and
(d) Preheat 150°C min
5M15 E Group 1730°C to 785°CNIL
6M8PWHT : NilNIL
7MX20PH: 250-300°C for
GTAW and 400-450
NIL
for SMAW
Post Heat:80-100°C
for 90 minutes
minimum
PWHT: 740°C -
760°C
8MX12 (t up to 52 mm)PH:220°C
PWHT: 725°C +/-
15°C
NIL
9M43950°C min(a) For design temperature less than 540°C
or
(b) for circumferential butt welds in pressure
parts with a nominal base metal thickness of
13 mm or less at the weld

Table structure read from the Gazette PDF, pages 574, 575. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
     Serial  Material group (as per         Table 3/5  PWHT not required under the following
      No.    Table 2/1)                       PWHT     conditions:
      (1)                                       (3)
                           (2)                                                   (4)
       1                             595°C min
             M1 Group 1, M1 Group 2                    (i) For All Product Forms:

     2       M3 Group 1              595°C min         (a) nominal weld thickness (t) ≤ 20 mm; and

     3 M4 Group 1                    650°C min         (b) If preheated to 95°C min when nominal
                                                       weld thickness (t) ≤ 20 mm and nominal base
     4 M5A Group 1 &                 675°C min         metal thickness ≤ 25 mm; and
             M5B Group 1
                                                       (c) C ≤ 0.25%;
     5 M15 E Group 1                 730°C to 785°C
     6 M8                                 PWHT : Nil   (ii) Only for tubes and pipes, if 0.25% < C ≤
                                                       0.3% and nominal thickness ≤ 9 mm; In case
                                                       of welded stays, diameter of stay is not used to
                                                       determine preheat requirements.

                                                       (a) For all product forms nominal wall
                                                       thickness (t) ≤ 16 mm except for tubes and
                                                       pipes t ≤ 13 mm & OD ≤ 127 mm; and

                                                       (b) C ≤ 0.25%

                                                       (a) For all product forms nominal base metal
                                                       thickness t ≤ 16 except for tubes and pipes
                                                       t ≤ 13 mm & OD ≤ 127 mm; and

                                                       (b) C ≤ 0.15%; and

                                                       (c) Preheat 120°C min

                                                       (a) For all product forms nominal base metal
                                                       thickness t ≤ 16 except for tubes t ≤ 13 mm &
                                                       OD ≤ 127 mm and for pipes t ≤ 13 mm & OD
                                                       ≤ 127 mm; and

                                                       (b) Cr ≤ 3%; and

                                                       (c) C ≤ 0.15%; and

                                                       (d) Preheat 150°C min

                                                       NIL

                                                       NIL

     7 MX20                          PH: 250-300°C for NIL
                                     GTAW and 400-450


                         for SMAW
                         Post Heat:80-100°C
                         for 90 minutes
                         minimum
                         PWHT: 740°C -
                         760°C

8  MX12 (t up to 52 mm)  PH:220°C                   NIL

                         PWHT: 725°C +/-

                         15°C

9 M43                    950°C min                  (a) For design temperature less than 540°C

                                                    or

                                                    (b) for circumferential butt welds in pressure
                                                    parts with a nominal base metal thickness of
                                                    13 mm or less at the weld

Notes-1:

(a)All the heat treatment ranges shall be aligned with the Qualified Welding Procedure.

(b)When pressure parts of two different M‐Number groups are joined by welding, the post weld heat treatment shall be as specified in Table 3/5 for the material requiring the higher post weld heat treatment temperature, except M-No. 8 group.

(c)Fillet welds, partial penetration welds, and full penetration welds through the tube or pipe thickness, attaching M-No. 4 or M-No. 5A tubes and pipe to headers of lower M‐Number material, may be post weld heat treated at the temperature specified in Table 3/5 for the lower M‐Number material provided the tubes or pipe comply with all the following conditions:

(i)a maximum specified chromium content of 3 percent

(ii)a maximum size of NPS 4 (DN 100)

(iii)a maximum thickness of 13 mm.

(iv)a maximum specified carbon content of not more than 0.15 percent

(d)When non-pressure parts are welded to pressure parts, the post weld heat treatment temperature of the pressure parts shall control. Pressure part welds and attachment welds using ferritic filler metals that have a specified chromium content of more than 3% shall receive a post weld heat treatment. The post weld heat treatment time and temperature used shall be not less than that shown in Table 3/5 for a base metal of equivalent analysis.

(e)The nominal thickness to be considered for determining Post Weld Heat Treatment and soaking time shall be defined as:

(i)For full penetration butt welds, the nominal thickness is the thinner of the parts being joined.

(ii)For full penetration corner welds, the nominal thickness is the depth of the weld.

(iii)For partial penetration groove and material repair welds, the nominal thickness is the depth of the weld. The total depth of partial or full penetration groove welds made from both sides shall be taken as the sum of the depth of both sides at a given location.

(iv)For fillet welds, the nominal thickness is the weld throat. When a fillet weld is used in conjunction with a groove weld, the nominal thickness is either the depth of the groove weld or the fillet throat dimension, whichever is greater.

(v)Except as stipulated in clause (vi) below, the nominal thickness is the depth of the groove, if present, through the shell or nozzle or reinforcing pad, or the throat of any fillet weld, whichever is greater.

(vi)When multiple openings form a ligament where the spacing between centres is less than twice the average diameter, the nominal thickness of a combination groove and fillet weld shall be the sum of the groove depth and fillet weld throat.

(vii)The thickness of the pressure part at the point of attachment where a non-pressure part is welded to a pressure part, in case of butt welds;

(viii)The thickness of the fillet weld at the point of attachment where a non –pressure part is welded to a pressure part, in case of fillet welds.

(f)When it is impractical to carry out PWHT at the temperature specified in Table III/5 for M1 and M3 materials, it is permissible to carry out PWHT at lower temperatures for longer periods of time in accordance with table 3/6 given below.

Table 3/6: Alternate PWHT requirements for Carbon and Low alloy steels

Serial No.Decrease in temperature below minimum specified temperature, °CMinimum holding time at decreased temperature, hour [Note(1)]Notes
(1)(2)(3)(4)
1282-
2564-
38310(2)
411120(2)

Table structure read from the Gazette PDF, page 576. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
     Serial    Decrease in temperature below    Minimum holding time at decreased    Notes
      No.    minimum specified temperature, °C             temperature, hour          (4)
                                                                [Note(1)]
      (1)                        (2)                                (3)

     1       28                                 2                                    -

     2       56                                 4                                    -

     3       83                                 10                                   (2)

     4       111                                20                                   (2)

Notes:

(1)Minimum holding time per 25 mm for thickness up to and including 50 mm. Add 15 min per 25 mm of thickness for thickness greater than 50 mm.

(2)These lower Post Weld Heat Treatment temperatures permitted only for M-No 1, Group 1 and 2 materials.

(g)Soaking during heating / SR (or PWHT) shall be as per below guidelines:

Original extracted text of the table above, continued (diagnostic)
Serial No. HT Cycle            \Table 3/7: Soaking                       Remarks
Serial No.HT CycleSoaking TimeRemarks
(1)(2)(3)(4)
1Hot Working/ NormalizingFor M5B, M-15E Gr1 (P91): 30 minutes
per 25 mm of “t” or 30 minutes min
whichever is greater & for all others 30
minutes per 25 mm of “t” or 15 minutes
min whichever is greater.
‘t’ is the product
thickness for Stress
relieving.
2SR/PWHT – Carbon Steels1 hour per 25 mm of “t” for “t” up to 50
mm with an additional 15 minutes for
every 25 mm above 50 mm (15 minutes
minimum).
‘t’ is nominal thickness
as per Note (b) of Table
3/5 for PWHT.
3SR/PWHT – Alloy Steels1 hour per 25 mm of “t” with below
mentioned minimum soaking times:
(M3 & M4) – 30 minutes minimum.
(M5A) – 60 minutes minimum except for
M5A pipes of OD ≤ 127mm and t ≤
13mm, which require only 30 minutes)
(M5B & M-15 E Gr 1) – 60 minutes
minimum
4MX202 hrs minimum for thickness below 60
mm and 3 hrs minimum for thickness
above 60 mm
5MX12 (t up to 52 mm)1 hour per 25 mm of ‘t’ - 30 minutes
minimum.
6SR/PWHT – Nickel Alloys1 hour per 25 mm of ‘t’ - 60 minutes
minimum.

Table structure read from the Gazette PDF, page 577. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
                                 Soaking Time

(1)                  (2)                            (3)                           (4)

1    Hot Working/ Normalizing  For M5B, M-15E Gr1 (P91): 30 minutes      ‘t’ is the product
                               per 25 mm of “t” or 30 minutes min        thickness for Stress
                               whichever is greater & for all others 30  relieving.
                               minutes per 25 mm of “t” or 15 minutes
                               min whichever is greater.

2    SR/PWHT – Carbon Steels   1 hour per 25 mm of “t” for “t” up to 50
                               mm with an additional 15 minutes for
                               every 25 mm above 50 mm (15 minutes
                               minimum).

3    SR/PWHT – Alloy Steels    1 hour per 25 mm of “t” with below
                               mentioned minimum soaking times:

                               (M3 & M4) – 30 minutes minimum.

                               (M5A) – 60 minutes minimum except for     ‘t’ is nominal thickness
                               M5A pipes of OD ≤ 127mm and t ≤           as per Note (b) of Table
                               13mm, which require only 30 minutes)      3/5 for PWHT.

                               (M5B & M-15 E Gr 1) – 60 minutes
                               minimum

4    MX20                      2 hrs minimum for thickness below 60
                               mm and 3 hrs minimum for thickness
                               above 60 mm

5    MX12 (t up to 52 mm)      1 hour per 25 mm of ‘t’ - 30 minutes
                               minimum.

6    SR/PWHT – Nickel Alloys   1 hour per 25 mm of ‘t’ - 60 minutes
Original extracted text of the table above, continued (diagnostic)
minimum.

(h)The temperature of the furnace at the time of placing the component for SR/PWHT shall not be higher than 425°C. The component shall be kept at SR/PWHT temperature to the minimum soaking time. After SR/PWHT the component shall be left to cool to in the furnace to a temperature not exceeding 425°C. After withdrawal from the furnace the part shall be allowed to cool in a still atmosphere.

(i)The rate of heating above 425°C and rate of cooling up to 425°C shall be as below. The rate of heating and rate of cooling should not exceed 335°C per hour divided by the thickness in inches, but in no case should it be more than 335°C per hour.

Notes 2:

(i)In case socket welded joints or other type of joints for carbon steel pipes, valves and fittings, PWHT is not required if the throat thickness of fillet weld does not exceed 20 mm or carbon content does not exceed 0.25%.

(ii)For carbon steel Headers and Mud boxes of water tube boilers, material having a maximum Carbon content of 0.25%, the Post Weld Heat Treatment requirement for tubes welded to Header is not mandatory when all the following conditions are fulfilled, namely:-

(a)The outer diameter (OD) of tubes is not more than 51 MM;

(b)The outer diameter of the Header is not more than 219.1 MM;

(c)The Header thickness is not more than 13 MM;

(d)A minimum pre-heat of 100°C is applied.

(iii)For Carbon steel, if the thickness of the small component of boiler exceeds 20 mm and the weld recess also exceeds 20 mm local stress relieving to the satisfaction of the Inspecting Authority shall be permitted.

(iv)Post-weld heat treatment in weld joints of carbon steel and low alloy steel may be exempted when heat treatment is not practical where inside is lined with special Stainless Steel which cannot be heated beyond 400°C (due to the associated problem of reduction of corrosion properties of such lining during heating to the temperature), when all the following conditions are satisfied –

(a)Built-up overlay welding (buttering is performed on both the welding edge bevels of the parts of the closing joint to be welded together. The buttering can be of:

(1)With Carbon Steel Electrode with low carbon (C) = 0.1 Percent max. (Ex: E7018-1) in case of Carbon Steel parts.

(2)With Stainless Steel Electrode E-309 or with Inconel electrode in case of low alloy steel parts.

(3)With low alloy steel electrodes, having carbon (C) = 0.12 percent maximum or with Inconel electrode in case of high strength low alloy steel parts having UTS greater than 56 kg/mm2 such as WB36, SA 533 Type B Cl 2;

(b)Buttering thickness shall be 15 mm minimum on the side where chip back is required to be done before re-welding and 8 mm minimum on the other side. Refer Figure given below:

Fig. 3/11

(c)Suitable pre-heat and other pass heating is applied during buttering:

(d)Individual parts are post-weld heat treated after buttering prior to welding the special stainless steel corrosion resistant liner plate or prior to applying final weld overlay of special corrosion resistant stainless steel lining;

(e)The final layer on the internal line side shall be compatible with liner material and final weld (carbon steel welding in carbon steel base metal, low alloy steel Inconel welding in case of high strength low alloy steel base metal and E309 Inconel welding in case of other low alloy steel base metals) on the base metal side shell be compatible with base metal in respect of mechanical properties. The welding procedure shall be established taking care of adequate toughness and ductility and the procedure approved by Inspecting Authority or Chief Inspector, as the case may be;

(f)Charpy – V Notch impact test is carried out at 20°C for:

(i)Base metal and heat affected zone,

(ii)Weld metal in case of Carbon Steel welding;

(g)Non-destructive testing as below (recommended):

(i)Magnetic particle test of weld bevels prior to buttering.

(ii)Dye-Penetrant test of buttering layer.

(iii)Dye-Penetrant test of rest of weld.

(iv)Dye-Penetrant test of final weld on internal liner side.

(v)Ultrasonic test of final weld after hydro test of the equipment with the closing seam.

Parts of this extracted text look garbled; read the Gazette page before using any value.

Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.

Figures cited in this regulation (1, exact crops of the Gazette)

Gazette Fig. 3/11
Fig. 3/11(no caption printed with this figure)
View Gazette page 578 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Independent explanation — not the law · draft · engineer review in progress

In short

Regulation 123 sets the post weld heat treatment (PWHT) rules. Table 3/5 gives PWHT temperatures by material group and the conditions under which PWHT is not required. Further notes and tables cover mixed materials, nominal thickness, alternative lower temperatures, soaking times, furnace practice and specific exemptions.

Key points

  • Table 3/5 covers material groups M1, M3, M4, M5A, M5B, M15E, M8, MX20, MX12 and M43 (groups as per Table 2/1). For each it gives the PWHT temperature (or preheat and post-heat for MX20 and MX12) and the thickness, carbon, chromium and preheat conditions for exemption. The extracted table layout is broken, so check the Gazette page for the exact values.
  • Notes 1: heat treatment ranges must align with the qualified welding procedure. When two M-number groups are joined, use the PWHT for the material needing the higher temperature (except the M-No. 8 group). For non-pressure attachments, the pressure part's PWHT temperature controls. Welds with ferritic filler of more than 3% chromium must receive PWHT.
  • Nominal thickness for PWHT and soaking is defined for butt, corner, groove, fillet and combined welds in Note (e).
  • Table 3/6 lets M1 and M3 materials be treated at lower temperatures for longer times where the specified temperature is impractical.
  • Table 3/7 gives soaking times for hot working/normalising and SR/PWHT by material.
  • Furnace practice: the furnace must not be hotter than 425°C when the part goes in; the part cools in the furnace to not more than 425°C, then in still air. Heating above and cooling down to 425°C must not exceed 335°C per hour divided by thickness in inches, and never more than 335°C per hour.

Watch out

  • Notes 2 exemptions: carbon steel socket welded and similar joints in pipes, valves and fittings need no PWHT if the fillet throat does not exceed 20 mm or carbon does not exceed 0.25%. Tube-to-header welds on carbon steel headers and mud boxes (max 0.25% carbon) are exempt only when tube OD is not more than 51 mm, header OD not more than 219.1 mm, header thickness not more than 13 mm and a preheat of at least 100°C is applied.
  • Local stress relieving to the Inspecting Authority's satisfaction is allowed for small carbon steel components where thickness and weld recess both exceed 20 mm.
  • Joints lined with special stainless steel that cannot be heated beyond 400°C may be exempted only if all the listed buttering, heat treatment, procedure approval and Charpy test (at 20°C) conditions are met.

Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.

Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).

Orientation hints (unverified)

These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.

Historical 1950-edition reg.Heading as OCR'dHeading similaritySource image
423Heat Treatment100%Chapter X (DPIIT scan), image 7
629Heat Treatment100%Chapter XV (DPIIT scan), image 2
94General requirements75%Chapter II (DPIIT scan), image 19
IBR 1950 regulation 423 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 423 page for its amendments.

Reg. 420, Reg. 421, Reg. 422, Reg. 423
TESTS FOR CLASS II FUSION WELDED SEAMS

Nick Break Test

The specimen shall be rectangular in section and cut transversely to the weld so as to have a width not less than one-and-half times its thickness. The slot shall be cut in one side of the specimen through the centre of the weld and perpendicular to the outer face of the vessel. The specimen shall than be broken in the weld and the fracture shall reveal a sound homogeneous-weld, substantially free from slag inclusions, porosity and coarse crystallinity.



Reg. 421
TESTS FOR CLASS II FUSION WELDED SEAMS

Retests

Should any of the tests fail, two retests shall be made on specimens cut from the same plate and both retests shall meet the specified requirements.



Reg. 422
TESTS FOR CLASS II FUSION WELDED SEAMS

Specimens after Tests

If required by the Inspecting Authority, the specimens after test shall be forwarded for examination.



Reg. 423
TESTS FOR CLASS II FUSION WELDED SEAMS

Heat Treatment

All fusion welded electrode boilers shall be stress-relieved by heat-treatment. The heat-treatment shall be in accordance with Regulation 267.

IBR 1950 regulation 94 as last published in the DPIIT web edition (archived 2019)

Unofficial archived copy, not verified; see the regulation 94 page for its amendments.

Reg. 94
MATERIALS OF CONSTRUCTION

COVERED ELECTRODES FOR METAL ARC WELDING OF MILD STEEL

General requirements

(1) Application.- The following Regulations apply to electrodes of sizes 3/32 inch (12 S.W.G.) and larger in diameter for metal arc welding of carbon steels having ultimate tensile strength not exceeding 33 tons per square inch and Sulphur and Phosphorus contents not greater than 0.06 per cent each. Electrodes less than 3/32 inch in diameter shall not be used in boilers.

The electrodes shall comply with the requirements of physical tests prescribed for each class.

Their characteristics and behaviour under ordinary working conditions shall be such that satisfactory weld deposits can be made by a welder of average skill and experience and that the following characteristics are also obtained:-

(a)

a relative ease in the control of the slag and weld metal during welding;

(b)

a good degree of stability of the arc and of the fusing of the covering;

(c)

no undue degree of spatter;

(d)

a fair rate of deposition and depth of penetration;

(e)

easy removability of the slag;

(f)

no undue tendency to under-cut;

(g)

a fair contour of the weld deposits; and

(h)

a low internal porosity of the weld metal.

(2) Classification.- The electrodes shall be classified into:

(a)

normal penetration electrodes for use in one or more welding positions; and

(b)

 

deep penetration electrodes for close unprepared butt-welding in the flat position and/or fillet welding, in the flat and horizontal – vertical positions.

(3) Manufacture.- Electrodes may be made by any method that shall yield a product conforming to the requirements of these Regulations.

(4) Size of Electrodes.- The nominal size of the electrodes shall refer to the diameter of the core wire and the length shall not exceed 18 inches. Provision shall be made for end or centre gripping.

The tolerances on the specified diameter of the core wire of the electrodes shall be plus or minus 0.002 inch.

(5) Covering.- The flux covering shall be sufficiently robust to withstand the normal conditions of transport, storage, handling and use, without damage and shall be uniform in thickness all over so that it fuses evenly. The variation in the thickness shall not exceed 3 per cent.

(6) (a) Packing and storage.- Electrodes shall be suitably packed to guard against damage during transportation. When stored, the electrodes shall be kept in their original bundles or packings in a dry store room and under such conditions, the electrodes shall for a period of at least six months be capable of giving results similar to those which they would have given on the date of their despatch from the manufacturer.

(b) Marking.- Each package shall be marked with the following information:-

Name of the Manufacturer.
Trade name of the Electrodes.
Size and quantity of Electrodes.
Batch number.
Recommended current range.
Classification as per Indian Boiler Regulations.

(7) Tests.- The electrodes shall be subjected to Initial tests, Periodic check tests and Production control to ensure that the requirements of these Regulations are fulfilled.

Electrodes intended for use with more than one type of current or polarity shall be tested using each type of current and polarity.

Where any test specimen fails to satisfy the requirements of any particular test, two further test specimens shall be prepared using the electrodes from the same batch and submitted to the same test.

The batch of electrodes shall be accepted as having passed the test provided that the tests of both the additional specimens are satisfactory.

(8) Test Certificates.- The manufacturers shall, when called upon, produce the results of the most recent Periodic check tests carried out within the preceding 12 months, on electrodes representative of the electrodes supplied.

Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Instrument
Indian Boiler Regulations, 2026 (made by the Central Boilers Board under s.40 of the Boilers Act, 2025)
Notification
F.No. P-30014/3/2021-Boiler dated 7 Aug 2026
Published
Gazette of India, Extraordinary, Part III Sec. 4, No. 596, 1 Oct 2026 (CG-DL-E-06102026-276813)
In force
1 Oct 2026 (reg. 1(3): date of publication in the Official Gazette)
Printed Gazette page
573–579
PDF page index
573–579 · open official e-Gazette PDF
Extraction
pdftotext layout mode, sequential regulation detector · text hash 79b009e3e2feb81c
Verification
Official text — not yet verified
Amendments checked
None known after 1 Oct 2026 as of build date (not a guarantee). Amendment log
How to cite

Indian Boiler Regulations, 2026, reg. 123, Regulation 123, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.573–579. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).

The citation refers to the government publication. Cite the Gazette, not this website.

Help improve this page

Engineers like you keep IBRsource accurate. Every checked correction or tip helps the next reader.