Indian Boiler Regulations, 2026 · Chapter 3 · Construction and Workmanship
Regulation 77. Preparation of plates
Not yet checked against the official Gazette; verify before relying on it.
77. Preparation of plates.─ (1)The edges of all plates and butt straps shall be machined or flame cut by machine and the caulking edges shall be bevelled to an angle not sharper than 20° to the plane of the plate and between 70° and 80°wherever practicable. Gusset Plates may be sheared except on those edges, which are to be welded.
(2)Plates which are to be flame-cut by machine without heat treatment or subsequent grinding or machining shall not have a carbon content higher than 0.25 per cent.
(3)Where the carbon content exceeds 0.25 percent, heat treatment, grinding or machining shall be carried out.
(4)The edges of all plates shall have a smooth finish.
(5)Before commencing welding of the joint (apart from tack welding), it shall be ascertained that the chamfered edges are in alignment and that the defects in alignment between the surfaces of the plates do not exceed as given in the table 3/1:
Table 3/1: ALIGNMENT TOLERANCE OF SECTIONS TO BE BUTT-WELDED
| Serial No. | Section Thickness(t), in mm | Direction of joints in cylindrical shells | |
|---|---|---|---|
| Longitudinal | Circumferential | ||
| 1 | Up to 13 mm incl. | ¼ t | ¼ t |
| 2 | Over 13 mm up to 19 mm | 3 mm | ¼ t |
| 3 | Over 19 mm and up to 38 | 3 mm | 5 mm |
| 4 | Over 38 mm and up to 51 mm | 3 mm | 3 mm |
| 5 | Over 51 mm | Lessor of t/16 or 9 mm | Lessor of t/8 or 19 mm |
Table structure read from the Gazette PDF, page 560. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Serial Section Thickness(t), in mm Direction of joints in cylindrical shells
No.
Longitudinal Circumferential
1 Up to 13 mm incl. ¼ t ¼ t
2 Over 13 mm up to 19 mm 3 mm ¼ t
3 Over 19 mm and up to 38 3 mm 5 mm
4 Over 38 mm and up to 51 mm 3 mm 3 mm
5 Over 51 mm Lessor of t/16 or 9 mm Lessor of t/8 or 19 mm(6)If plate edges of unequal thickness are abutted and the difference between the surfaces exceeds the limit mentioned as above on either side, the thicker plate shall be thinned to a smooth taper for a distance not less than 4 times the offset including, if so desired, the width of the weld. In longitudinal joints, the middle line of the plates shall be in alignment within 10 per cent of the thickness of the thicker plate with a maximum of 3 mm.
Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.
In short
Regulation 77 sets how plate edges are prepared and aligned before welding, including the alignment tolerances for butt-welded sections.
Key points
- (1) Edges of plates and butt straps are machined or machine flame cut. Caulking edges are bevelled no sharper than 20° to the plate, and between 70° and 80° wherever practicable. Gusset plates may be sheared, except on edges to be welded.
- (2), (3) Plates flame-cut by machine with no later heat treatment, grinding or machining must not exceed 0.25 per cent carbon. Above that, heat treatment, grinding or machining is required.
- (4) All plate edges must have a smooth finish.
- (5) Before welding (other than tack welding), check that chamfered edges are aligned. Misalignment must stay within Table 3/1, which gives limits by section thickness for longitudinal and circumferential joints in cylindrical shells.
- (6) Where plates of unequal thickness are joined and the surface difference exceeds those limits, the thicker plate is tapered over at least 4 times the offset (the weld width may be included). In longitudinal joints, the plate middle lines must align within 10 per cent of the thicker plate's thickness, with a maximum of 3 mm.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
| Historical 1950-edition reg. | Heading as OCR'd | Heading similarity | Source image |
|---|---|---|---|
| 33 | Plates | 100% | Chapter II (DPIIT scan), image 3 |
| 118 | Tube Plates | 71% | Chapter III (DPIIT scan), image 2 |
| 634 | Tube plates | 71% | Chapter XV (DPIIT scan), image 3 |
IBR 1950 regulation 33 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 33 page for its amendments.
| Reg. 33 MATERIALS OF CONSTRUCTION COPPER PLATES, STAY AND RIVET BARS |
| (a) Process.- The copper shall be fire-refined or electrolytic and hot-rolled from suitable cakes. (b) Chemical Composition.- The chemical composition of the plates shall be as follows:-
(c) Freedom from defects.- The plates shall be clean, smooth and free from defects and shall have a workmanlike finish. They shall be thoroughly annealed. (d) Rolling Margin.- No plate shall be under the specified thickness at any part, not more than 5% over the calculated weight. The scrap margin, partly sheared and left attached, shall be not less than 3 inches at the ends and 1½ inches at each side. (e) Tensile Tests.- One tensile test shall be taken from each plate as rolled. The tensile breaking strength, from Standard Test Piece A, shall not be less than 14 tons per sq. inch with an elongation of not less than 35%. (f) Hot and Cold Bend tests.- One hot (temperature between 1200°F and 1400°F) and one cold bend test shall be taken from each plate as rolled. For either hot or cold bend tests, the test piece shall withstand being doubled over without fracture until the sides are touching and parallel. |
IBR 1950 regulation 118 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 118 page for its amendments.
| Reg. 118, Reg. 119, Reg. 120 END PLATES
Tube Plates Parts of flat tube plates within the tube nests
Reg. 120 END PLATES Flanging of End Plates All flanges shall be a good fit to the shell and flues. Flogging and/or hammering in the fitting of these parts is prohibited. The caulking edges of all flanged plates shall be machined or machine gas cut. |
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Indian Boiler Regulations, 2026, reg. 77, Regulation 77, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.560. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.