BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Indian Boiler Regulations, 2026 · Chapter 7 · Pipes and Fittings

Regulation 263. Welded on flanges

Official text — not yet verifiedGazette 1 Oct 2026 · printed pp. 655–657TableFigure referenced

Not yet checked against the official Gazette; verify before relying on it.

Reproduced from the Gazette of India · verification status above

263. Welded on flanges.─ (1) Where flanges are welded on, the welding shall be done by the oxy-acetylene or metal arc process; the latter with covered electrodes which shall comply with regulations 71 to76.

(2)(a)The proportion of the weld shall be as indicated in the Figs.7/10 to 7/34(part V of this chapter) for the following types as mentioned in the Table below,-

Type1. Welding Neck Flange, Fig.7/10.
2. ‘Face and Back’ welded – on flange for metal arc welding. fig. 7/26.
3. ‘Bore and Back’ welded- on flange for metal arc welding. fig. 7/27 and 7/28.
4. ‘Face and Fillet’ welded- on flange for metal arc welding. fig. 7/29.
5. ‘Bore and Fillet welded- on flange for metal arc welding. fig. 7/30 and 7/31.
6. ‘Slip on’ welded- on flange for metal arc welding. fig. 7/32.
7. ‘Slip on’ welded- on bossed flange for oxy-acetylene welding. fig. 7/33.
8. Socket welded flange, Fig.7/34.
The Flange shall not be a tight fit on the pipe.

Table structure read from the Gazette PDF, page 655. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
Type               1. Welding Neck Flange, Fig.7/10.
                   2. ‘Face and Back’ welded – on flange for metal arc welding. fig. 7/26.
                   3. ‘Bore and Back’ welded- on flange for metal arc welding. fig. 7/27 and 7/28.
                   4. ‘Face and Fillet’ welded- on flange for metal arc welding. fig. 7/29.
                   5. ‘Bore and Fillet welded- on flange for metal arc welding. fig. 7/30 and 7/31.
                   6. ‘Slip on’ welded- on flange for metal arc welding. fig. 7/32.
                   7. ‘Slip on’ welded- on bossed flange for oxy-acetylene welding. fig. 7/33.
                   8. Socket welded flange, Fig.7/34.

                   The Flange shall not be a tight fit on the pipe.

(b)The maximum clearance between the bore of the flange and the outside diameter of the pipe shall be 3 mm at any point, and the sum of clearance diametrically opposite shall not exceed 5 mm.

Note: All dimensions shown in the figures of types 1 to 7 relate to finished sizes. The design conditions for each type are as follows:
Types 1, 2 and 3 flanges for all maximum allowable working pressure and temperature conditions.

Types 4 and 5 flanges for all pressure conditions up to and including 42 kg/cm2 (g) and design temperature not exceeding 399°C.
Types 6 and 7 flanges for all pressure conditions up to and including 17.6 kg/cm2 (g) and temperature not exceeding 399°C except that Bossed flanges of type 6 shall not be used on pipes over 304 mm in nominal bore, nor Bossed flanges of type 7 on pipes 152 mm in nominal bore.

Type 8 flanges for all maximum allowable working pressure and temperature conditions and this type shall be used only for pipes up to and including 51 mm nominal bore. These flanges shall not be used where severe erosion or corrosion is expected to occur.

(3)Type 1,2,3,4 and 5 Carbon Steel types flanges welded on by the metal arc process shall have the welds stress relieved where the design depth of the weld recess is greater than 20 mm and all welds joining flanges to alloy steel pipes shall be stress relieved.

(4)Where type 1 flanges are attached by oxy-acetylene welding, the welds shall be normalised in accordance with the following requirements:

(a)Welds in mild steel pipes shall be normalised by heating the metal to a temperature between 900° and 950°C, the temperature then being maintained for not less than two minutes for pipes up to and including 102 mm bore, and for not less than five minutes for pipes over 102 mm bore.

(b)Welds in pipes made from the alloy steel shall be normalised by heating the metal to a temperature between 925° and 975°C, the temperature then being maintained for not less than two minutes for pipes up to and including 102 mm bore, and for not less than five minutes for pipes over 102 mm bore.

(c)The higher temperatures of between 950° and 975°C, shall be used for alloy steels having a carbon content up to and including 0.12 percent and the lower temperatures of between 925° and 950°C shall be used for alloy steels having a carbon content of more than 0.12 percent.

(d)After normalising the joint shall be covered with a suitable muff or asbestos cloth to ensure slow and even cooling.

(e)The normalising of welds in pipes up to 102 mm bore may be carried out with welding flames the temperature being judged with the aid of a colour card, or measured by means of one or more thermo-couples or an optical pyrometer.

(f)The normalising of welds in pipes over 102 mm bore shall preferably be carried out in a portable pipe normalising furnace or muffle, the temperature being measured by means of one or more thermo-couples or an optical pyrometer.

(g)The width of the zone to be heat treated to the specified temperature shall extend at least 13 mm on either side of the weld reinforcement.

(5)The procedure to be observed in the stress relieving of welds shall be in accordance with regulation 123 and stress relieving shall be carried out by any of the following methods:-

(a)(i) Local heating using a portable muffle furnace, induction coils or other suitable appliances and due care shall be taken to apply heat uniformly over the area to be treated.

(ii)The use of procedures not providing adequate control such as manual operated gas torches are not permissible.

(iii)The temperature shall be measured by the thermo-couples pinned, welded or otherwise suitably attached to the surface of the pipe and where necessary, protection from flame impingement shall be taken.

(b)The temperature of the joint during heating in a stationary industrial furnace shall be measured by thermo-couples appropriately placed within the furnace as to give a true measure of the joint temperature.

Parts of this extracted text look garbled; read the Gazette page before using any value.

Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.

Referenced provisions

Reg. 71 · Reg. 76 · Reg. 123

Figures cited in this regulation (25, exact crops of the Gazette)

Gazette Fig. 7/10: Welding Neck Flange
Fig. 7/10Welding Neck Flange
View Gazette page 669 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/11: Plain Vee for Use with Backing Ring
Fig. 7/11Plain Vee for Use with Backing Ring
View Gazette page 669 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/12: Double Angle Vee for Use with Backing Ring
Fig. 7/12Double Angle Vee for Use with Backing Ring
View Gazette page 669 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/13: Normal preparation U-Groove for use with backing ring
Fig. 7/13Normal preparation U-Groove for use with backing ring
View Gazette page 670 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/14: Permissible Alternative Preparation for Vertical or Nearly Vertical Pipe U-Groove for Use with Backing Ring
Fig. 7/14Permissible Alternative Preparation for Vertical or Nearly Vertical Pipe U-Groove for Use with Backing Ring
View Gazette page 670 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/15: Preparation of Groove for Use with Taper Backing Ring and Double Root Run
Fig. 7/15Preparation of Groove for Use with Taper Backing Ring and Double Root Run
View Gazette page 670 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/16: Groove for Use with Recessed Backing Ring
Fig. 7/16Groove for Use with Recessed Backing Ring
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/17: Groove for User with Recessed Backing Ring
Fig. 7/17Groove for User with Recessed Backing Ring
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/18: Normal Preparation Double Angle Vee for Use with Oxy-Acetylene Base Run
Fig. 7/18Normal Preparation Double Angle Vee for Use with Oxy-Acetylene Base Run
View Gazette page 670 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/19: Double Angle Vee for Use with Oxy-Acetylene Base Run
Fig. 7/19Double Angle Vee for Use with Oxy-Acetylene Base Run
View Gazette page 670 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/20: U-Groove for Use With Oxy-Acetylene Base Run
Fig. 7/20U-Groove for Use With Oxy-Acetylene Base Run
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/21: U-Groove for Use With Oxy-Acetylene Base Run
Fig. 7/21U-Groove for Use With Oxy-Acetylene Base Run
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/22: Plain Vee for Use With Oxy-Acetylene Base Run
Fig. 7/22Plain Vee for Use With Oxy-Acetylene Base Run
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/23: Plain Vee for Use Without Backing Ring
Fig. 7/23Plain Vee for Use Without Backing Ring
View Gazette page 672 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/24: Plain Vee for Use Without Backing Ring
Fig. 7/24Plain Vee for Use Without Backing Ring
View Gazette page 671 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/25: Single U for Use Without Backing Ring
Fig. 7/25Single U for Use Without Backing Ring
View Gazette page 672 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/26
Fig. 7/26(no caption printed with this figure)
View Gazette page 672 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/27
Fig. 7/27(no caption printed with this figure)
View Gazette page 672 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/28
Fig. 7/28(no caption printed with this figure)
View Gazette page 673 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/29
Fig. 7/29(no caption printed with this figure)
View Gazette page 674 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/30
Fig. 7/30(no caption printed with this figure)
View Gazette page 673 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/31
Fig. 7/31(no caption printed with this figure)
View Gazette page 674 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/32: For Clearance Between Flange Bore & O.D. of Pipe [See regulation263(2)]
Fig. 7/32For Clearance Between Flange Bore & O.D. of Pipe [See regulation263(2)]
View Gazette page 674 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Gazette Fig. 7/33: For Clearance Between Flange Bore & O.D. of Pipe [see regulation263(2)]
Fig. 7/33For Clearance Between Flange Bore & O.D. of Pipe [see regulation263(2)]
View Gazette page 675 · figure catalogue
Reconstructed CAD: DXF · SVG · Preview (redrawn, checked against the print; technical review pending)
Independent explanation — not the law · draft · engineer review in progress

In short

Regulation 263 covers welded-on pipe flanges: welding process, the eight permitted flange types and their limits, fit-up clearance, and normalising or stress relieving of the welds.

Key points

  • (1) Welding by oxy-acetylene or metal arc. Metal arc electrodes must comply with regulations 71 to 76.
  • (2)(a) Weld proportions follow Figs. 7/10 to 7/34 for eight types: welding neck, face and back, bore and back, face and fillet, bore and fillet, slip on, slip on bossed (oxy-acetylene) and socket welded. The flange must not be a tight fit on the pipe.
  • (2)(b) Clearance between flange bore and pipe OD: at most 3 mm at any point, and diametrically opposite clearances must not total more than 5 mm.
  • Type limits: types 1, 2, 3 and 8 for all pressures and temperatures. Types 4 and 5 up to and including 42 kg/cm2 (g) and 399°C. Types 6 and 7 up to and including 17.6 kg/cm2 (g) and 399°C. Type 8 only up to and including 51 mm nominal bore.
  • (3) Metal arc welds on carbon steel types 1 to 5 must be stress relieved where the weld recess is deeper than 20 mm. All welds joining flanges to alloy steel pipes must be stress relieved.
  • (4) Oxy-acetylene welded type 1 flanges must have welds normalised: mild steel at 900° to 950°C, alloy steel at 925° to 975°C. Hold not less than two minutes for bores up to and including 102 mm and five minutes above. Higher alloy range (950° to 975°C) for carbon up to and including 0.12 percent; lower (925° to 950°C) above it. The heated zone extends at least 13 mm either side of the weld reinforcement, followed by slow, even cooling.
  • (5) Stress relieving follows regulation 123, by controlled local heating with attached thermo-couples, or in a stationary furnace.

Watch out

  • Bossed type 6 flanges must not be used on pipes over 304 mm nominal bore. The limit for bossed type 7 flanges (152 mm nominal bore) reads incompletely; check the Gazette page.
  • Type 8 must not be used where severe erosion or corrosion is expected.
  • Manually operated gas torches are not permissible for stress relieving.

Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.

Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).

Orientation hints (unverified)

These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.

Historical 1950-edition reg.Heading as OCR'dHeading similaritySource image
410Flanges100%Chapter X (DPIIT scan), image 4
IBR 1950 regulation 410 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 410 page for its amendments.

Reg. 410, Reg. 411, Reg. 412
RIVETED STEEL BOILERS

Flange-Thickness and Drilling

The thickness and drilling of flanges of standpipes shall be in accordance with the Appendix (E).



Reg. 411
RIVETED STEEL BOILERS

Pads

These shall comply with Regulation 155.



Reg. 412
RIVETED STEEL BOILERS

Unstayed Flat-End Plates

The working pressure of unstayed flat-end plates shall be determined by the following formula:

W.P. = 2S(t-2)² Eqn. (98)
D²

Where,

t = thickness of plate in thirty-seconds of an inch.
W.P. = Working pressure in pounds per square inch.
D = Diameter in inches of the pitch circle of the bolts or rivets when the plate is attached to an outside flange or the internal diameter of the shell when the plate is attached to an inside flange.
S = Minimum tensile stress of the plate in tons per square inch.

In no case shell the thickness of an unstayed flat-end plate be less than 3/8 inch.

Where an unstayed flat-end plate is pierced for electrodes or other fittings by openings having a diameter not greater than 2 ½ inches and the pitch of the openings in inches is not less than four times the diameter of the openings in inches, compensation is not required.

Where the diameter of the openings in an unstayed flat-end plate is greater than 2 ½ inches or the pitch in inches is less than four times the diameter of the openings, adequate compensation shall be provided in the manner described in Regulations 170, 171 and 186.

Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Instrument
Indian Boiler Regulations, 2026 (made by the Central Boilers Board under s.40 of the Boilers Act, 2025)
Notification
F.No. P-30014/3/2021-Boiler dated 7 Aug 2026
Published
Gazette of India, Extraordinary, Part III Sec. 4, No. 596, 1 Oct 2026 (CG-DL-E-06102026-276813)
In force
1 Oct 2026 (reg. 1(3): date of publication in the Official Gazette)
Printed Gazette page
655–657
PDF page index
655–657 · open official e-Gazette PDF
Extraction
pdftotext layout mode, sequential regulation detector · text hash 21f80b4e7aafb3f8
Verification
Official text — not yet verified
Amendments checked
None known after 1 Oct 2026 as of build date (not a guarantee). Amendment log
How to cite

Indian Boiler Regulations, 2026, reg. 263, Regulation 263, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.655–657. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).

The citation refers to the government publication. Cite the Gazette, not this website.

Help improve this page

Engineers like you keep IBRsource accurate. Every checked correction or tip helps the next reader.