Indian Boiler Regulations, 2026 · Chapter 2 · Materials of Construction
Regulation 51. Process of manufacture
Not yet checked against the official Gazette; verify before relying on it.
51. Process of manufacture.– (1) The steel used for castings shall be made by an Open Hearth or Electric Furnace or any other process which gives steel having equivalent properties.
(2)The steel shall comply with the chemical composition specified in the Table 2/32.
Table 2/32: Chemical composition (%)
| Serial No. | Grade | Carbon(C) | Manganese (Mn) | Phosphorus (P) | Sulphur(S) | Silicon(Si) | Chromium (Cr) | Nickel(Ni) | Molybdenum(Mo) | Vanadium (V) | Nitrogen (N) | Others |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| (1) | (2) | (3) | (4) | (5) | (6) | (7) | (8) | (9) | (10) | (11) | (12) | (13) |
| 1. | SA 352 LCB | 0.30 | 1.00 | 0.04 | 0.045 | 0.60 | 0.50 | 0.50 | 0.20 | 0.03 | - | Cu-0.30 |
| 2. | SA 216 WCB | 0.30 | 1.20 | 0.04 | 0.045 | 0.60 | 0.50 | 0.50 | 0.20 | 0.03 | - | Cu-0.30 |
| 3. | SA 216 WCC | 0.25 | 1.20 | 0.04 | 0.045 | 0.60 | 0.50 | 0.50 | 0.20 | 0.03 | - | Cu-0.30 |
| 4. | SA 352 LCC | 0.25 | 1.20 | 0.04 | 0.045 | 0.60 | 0.50 | 0.50 | 0.50 | 0.03 | Cu-0.30 | |
| 5. | SA 217 WC6 | 0.05–0.20 | 0.50–0.80 | 0.04 | 0.045 | 0.60 | 1.00–1.50 | 0.50 | 0.45–0.65 | - | - | Cu-0.50 W-0.10 |
| 6. | SA 217 WC9 | 0.05–0.18 | 0.40–0.70 | 0.04 | 0.045 | 0.60 | 2.00–2.75 | 0.50 | 0.90–1.20 | - | - | Cu-0.50 W-0.10 |
| 7. | SA 217 C12A | 0.08–0.12 | 0.30–0.60 | 0.030 | 0.010 | 0.20–0.50 | 8.0–9.5 | 0.40 | 0.85–1.05 | 0.18–0.25 | 0.030– 0.070 | Nb- 0.060–0.10 Al- 0.02 Ti- 0.01 Zr- 0.01 |
| 8. | SA 351 CF8 | 0.08 | 1.50 | 0.040 | 0.040 | 2.00 | 18.0-21.0 | 8.0-11.0 | 0.50 | - | - | - |
| 9. | SA 351 CF8M | 0.08 | 1.50 | 0.040 | 0.040 | 1.50 | 18.0–21.0 | 9.0–12.0 | 2.0–3.0 | - | - | - |
| 10. | SA 351 CF8C | 0.08 | 1.50 | 0.040 | 0.040 | 2.00 | 18.0–21.0 | 9.0-12.0 | 0.50 | - | - | - |
Table structure read from the Gazette PDF, page 539. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Serial No. Grade Carbon(C) Manganese Phosphorus Sulphur(S) Silicon(Si) Chromium Nickel(Ni) Molybden Vanadium Nitrogen Others
(1) (2) (Mn) (P) (Cr) um(Mo) (V) (N) (13)
1.
2. (3) (4) (5) (6) (7) (8) (9) (10) (11) (12)
3.
4. SA 352 LCB 0.30 1.00 0.04 0.045 0.60 0.50 0.50 0.20 0.03 - Cu-0.30
5. 0.045 0.50 -
6. SA 216 WCB 0.30 1.20 0.04 0.045 0.60 0.50 0.50 0.20 0.03 - Cu-0.30
7. 0.045 0.50
SA 216 WCC 0.25 1.20 0.04 0.045 0.60 0.50 0.50 0.20 0.03 - Cu-0.30
8. 0.045 0.50 -
9. SA 352 LCC 0.25 1.20 0.04 0.60 0.50 0.50 0.03 Cu-0.30
10. 0.010 0.40 0.030– Cu-0.50
SA 217 WC6 0.05–0.20 0.50–0.80 0.04 0.60 1.00–1.50 0.45–0.65 - 0.070 W-0.10
0.040 8.0-11.0 Cu-0.50
SA 217 WC9 0.05–0.18 0.40–0.70 0.04 0.040 0.60 2.00–2.75 0.90–1.20 - - W-0.10
0.040
SA 217 C12A 0.08–0.12 0.30–0.60 0.030 0.20–0.50 8.0–9.5 0.85–1.05 0.18–0.25 Nb- 0.060–0.10
Al- 0.02
SA 351 CF8 0.08 1.50 0.040 2.00 18.0-21.0 0.50 - Ti- 0.01
Zr- 0.01
-
SA 351 CF8M 0.08 1.50 0.040 1.50 18.0–21.0 9.0–12.0 2.0–3.0 - - -
SA 351 CF8C 0.08 1.50 0.040 2.00 18.0–21.0 9.0-12.0 0.50 - - -Note: 1. Maximum when single values specified
2. A carbon content not exceeding 0.3% may be subjected to the agreement between the boiler maker and the inspecting Authority.
Parts of this extracted text look garbled; read the Gazette page before using any value.
Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.
In short
Steel for castings is made by an Open Hearth or Electric Furnace process, or any process giving equivalent properties, and must meet the chemical composition in Table 2/32.
Key points
- Table 2/32 covers SA 352, SA 216, SA 217 and SA 351 grades. Single values are maximums.
- A carbon content not exceeding 0.3% may be subject to agreement between the boiler maker and the Inspecting Authority.
Watch out
- Table 2/32 is misaligned in the extracted text. Check the Gazette page for the exact limits.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
| Historical 1950-edition reg. | Heading as OCR'd | Heading similarity | Source image |
|---|---|---|---|
| 348 | Method of manufacture, Heat treatment and Marking | 78% | Chapter VIII (DPIIT scan), image 3 |
Amendment history of the candidate IBR 1950 regulation: Reg. 348 (1 amendment)
IBR 1950 regulation 348 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 348 page for its amendments.
| Reg. 348 Method of manufacture, Heat treatment and Marking
|
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.



Indian Boiler Regulations, 2026, reg. 51, Regulation 51, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.538–540. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.