Indian Boiler Regulations, 2026 · Chapter 2 · Materials of Construction
Regulation 60. Tensile strength
Not yet checked against the official Gazette; verify before relying on it.
60. Tensile strength.–(1) The tensile strength of the material shall conform with mechanical properties as per
Table 2/36 of this sub-regulation.
Table 2/36
| Serial No. | Grade | Mechanical Properties (minimum, when single value specified) | ||
|---|---|---|---|---|
| TS MPa (kg/mm2) | YS MPa (kg/mm2) | % Elongation on GL = 50 mm min*. | ||
| (1) | (2) | (3) | (4) | (5) |
| 1. | SA 266 Gr1 | 415-585 (42.3–59.6) | 205 (21) | 23 |
| 2. | SA 266 Gr2 | 485–655 (49.5–66.8) | 250 (25.5) | 20 |
| 3. | SA 266 Gr3 | 515–690 (52.5–70.4) | 260 (26.5) | 19 |
| 4. | SA 350 LF1 | 415-585 (42.3–59.6) | 205 (21) | 25 |
| 5. | SA 350 LF2 | 485-655 (49.5-66.8) | 250 (25.5) | 22 |
| 6. | SA 105 | 485 (49.5) | 250 (25.5) | 30 |
| 7. | SA 182 F1 | 485 (49.5) | 275 (28) | 20 |
| 8. | SA 182 F2 | 485 (49.5) | 275 (28) | 20 |
| 9. | SA 182 F11 Cl 1 | 415 (42.3) | 205 (21) | 20 |
| 10. | SA 182 F11 Cl 2 | 485 (49.5) | 275 (28) | 20 |
| 11. | SA 182 F11 Cl 3 | 515 (52.5) | 310 (31.6) | 20 |
| 12. | SA 182 F12 Cl 1 | 415 (42.3) | 220 (22.4) | 20 |
| 13. | SA 182 F12 Cl 2 | 485 (49.5) | 275 (28) | 20 |
| 14. | SA 182 F22 Cl 1 | 415 (42.3) | 205 (21) | 20 |
| 15. | SA 182 F22 Cl 3 | 515 (52.5) | 310 (31.6) | 20 |
| 16. | SA 182 F5 | 485 (49.5) | 275 (28) | 20 |
| 17. | SA 182 F9 | 585 (59.6) | 380 (38.7) | 20 |
| 18. | SA 182 F91 | 620 (63.2) | 415 (42.3) | 20 |
| 19. | SA 182 F304 | 515 (52.5) | 205 (21) | 30 |
| 20. | SA 182 F304H | 515 (52.5) | 205 (21) | 30 |
| 21. | SA 182 F304L | 485 (49.5) | 170 (17.3) | 30 |
| 22. | SA 182 F316 | 515 (52.5) | 205 (21) | 30 |
| 23. | SA 182 F316H | 515 (52.5) | 205 (21) | 30 |
| 24. | SA 182 F316L | 485 (49.5) | 170 (17.3) | 30 |
| 25. | SA 182 F321 | 515 (52.5) | 205 (21) | 30 |
| 26. | SA 234 WPB | 415 (42.3) | 240 (24.5) | 22 |
| 27. | SA 234 WPC | 485 (49.5) | 275 (28) | 22 |
| 28. | SA 182 F321H | 515 (52.5) | 205 (21) | 30 |
| 29. | SA 182 F347H | 515 (52.5) | 205 (21) | 30 |
| 30. | SA 234 WP11 Cl 1 | 415-585 (42.3–59.6) | 205 (21) | 22 |
| 31. | SA 234 WP12 Cl 1 | 415-585 (42.3–59.6) | 220 (22.4) | 22 |
| 32. | SA 234 WP22 Cl 1 | 415-585 (42.3–59.6) | 205 (21) | 22 |
| 33. | SA 234 WP5 Cl1 | 415-585 (42.3–59.6) | 205 (21) | 22 |
| 34. | SA 234 WP9 Cl1 | 415-585 (42.3–59.6) | 205 (21) | 22 |
| 35. | SA 234 WP91 | 585–760 (59.6–77.5) | 415 (42.3) | 20 |
| 36. | SA 336 F11 Cl 1 | 415-585 (42.3–59.6) | 205 (21) | 20 |
| 37. | SA 336 F11 Cl 2 | 485–660 (49.5–67.3) | 275 (28) | 20 |
| 38. | SA 336 F11 Cl 3 | 515–690 (52.5–70.4) | 310 (31.6) | 18 |
| 39. | SA 336 F12 | 485–660 (49.5–67.3) | 275 (28) | 20 |
| 40. | SA 336 F5 | 415-585 (42.3–59.6) | 250 (25.5) | 20 |
| 41. | SA 336 F9 | 585–760 (60.7–77.5) | 380 (38.7) | 20 |
| 42. | SA 336 F91 | 620–760 (63.2–77.5) | 415 (42.3) | 20 |
| 43. | SB 564 N06617 SB 166 N06617 | 655 (66.8) | 241 (24.6) | 35 |
Table structure read from the Gazette PDF, pages 546, 547. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Serial Grade Mechanical Properties (minimum, when single value specified)
No.
TS YS % Elongation on
(1) (2) MPa (kg/mm2) MPa (kg/mm2) GL = 50 mm
min*.
1. SA 266 Gr1 (3) (4) (5)
415-585 (42.3–59.6) 205 (21) 23
2. SA 266 Gr2 485–655 (49.5–66.8) 250 (25.5) 20
3. SA 266 Gr3 515–690 (52.5–70.4) 260 (26.5) 19
4. SA 350 LF1 415-585 (42.3–59.6) 205 (21) 25
5. SA 350 LF2 485-655 (49.5-66.8) 250 (25.5) 22
6. SA 105 485 (49.5) 250 (25.5) 30
7. SA 182 F1 485 (49.5) 275 (28) 20
8. SA 182 F2 485 (49.5) 275 (28) 20
9. SA 182 F11 Cl 1 415 (42.3) 205 (21) 20
10. SA 182 F11 Cl 2 485 (49.5) 275 (28) 20
11. SA 182 F11 Cl 3 515 (52.5) 310 (31.6) 20
12. SA 182 F12 Cl 1 415 (42.3) 220 (22.4) 20
13. SA 182 F12 Cl 2 485 (49.5) 275 (28) 20
14. SA 182 F22 Cl 1 415 (42.3) 205 (21) 20
15. SA 182 F22 Cl 3 515 (52.5) 310 (31.6) 20
16. SA 182 F5 485 (49.5) 275 (28) 20
17. SA 182 F9 585 (59.6) 380 (38.7) 20
18. SA 182 F91 620 (63.2) 415 (42.3) 20
19. SA 182 F304 515 (52.5) 205 (21) 30
20. SA 182 F304H 515 (52.5) 205 (21) 30
21. SA 182 F304L 485 (49.5) 170 (17.3) 30
22. SA 182 F316 515 (52.5) 205 (21) 30
23. SA 182 F316H 515 (52.5) 205 (21) 30
24. SA 182 F316L 485 (49.5) 170 (17.3) 30
25. SA 182 F321 515 (52.5) 205 (21) 30
26. SA 234 WPB 415 (42.3) 240 (24.5) 22
27. SA 234 WPC 485 (49.5) 275 (28) 22
28. SA 182 F321H 515 (52.5) 205 (21) 30
29. SA 182 F347H 515 (52.5) 205 (21) 30
30. SA 234 WP11 Cl 1 415-585 (42.3–59.6) 205 (21) 22
31. SA 234 WP12 Cl 1 415-585 (42.3–59.6) 220 (22.4) 22
32. SA 234 WP22 Cl 1 415-585 (42.3–59.6) 205 (21) 22
33. SA 234 WP5 Cl1 415-585 (42.3–59.6) 205 (21) 22
34. SA 234 WP9 Cl1 415-585 (42.3–59.6) 205 (21) 22
35. SA 234 WP91 585–760 (59.6–77.5) 415 (42.3) 20
36. SA 336 F11 Cl 1 415-585 (42.3–59.6) 205 (21) 20
37. SA 336 F11 Cl 2 485–660 (49.5–67.3) 275 (28) 20
38. SA 336 F11 Cl 3 515–690 (52.5–70.4) 310 (31.6) 18
39. SA 336 F12 485–660 (49.5–67.3) 275 (28) 20
40. SA 336 F5 415-585 (42.3–59.6) 250 (25.5) 20
41. SA 336 F9 585–760 (60.7–77.5) 380 (38.7) 20
42. SA 336 F91 620–760 (63.2–77.5) 415 (42.3) 20
43. SB 564 N06617 655 (66.8) 241 (24.6) 35
SB 166 N06617*The tensile test specimen shall be as per the relevant material specifications.
(2)The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength.
(3)The minimum values of the stress at proof limit 0.2% at elevated temperature (Et) may be calculated by multiplying the minimum specified tensile strength of the material at room temperature (R20) by the value of the ratio Et/R20 given in the Table 2/5 under regulation 37.
Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.
In short
Regulation 60 sets the tensile requirements for forgings.
Key points
- (1) Tensile properties must meet Table 2/36, which gives tensile strength, yield strength (MPa, with kg/mm2) and minimum % elongation on a 50 mm gauge length for each grade. See the Official text tab for the values.
- (2) The upper yield point at room temperature must be at least 50% of the specified minimum tensile strength.
- (3) The minimum 0.2% proof stress at elevated temperature (Et) may be calculated from the room-temperature tensile strength (R20) using the Et/R20 ratios in Table 2/5 of regulation 37.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
| Historical 1950-edition reg. | Heading as OCR'd | Heading similarity | Source image |
|---|---|---|---|
| 91 | Tensile test | 79% | Chapter II (DPIIT scan), image 18 |
| 83 | Tensile Tests | 76% | Chapter II (DPIIT scan), image 16 |
| 260 | Tensile Tests | 76% | Chapter V (DPIIT scan), image 6 |
Amendment history of the candidate IBR 1950 regulations: Reg. 260 (1 amendment)
IBR 1950 regulation 91 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 91 page for its amendments.
| Reg. 91 MATERIALS OF CONSTRUCTION GENERAL GREY IRON CASTINGS (GRADE A) Tensile test |
| A tensile test bar machined to the dimensions shown in Regulation 88(b) and tested with either plain or screwed ends must show a breaking strength of not less than that shown in the following table:-
|
IBR 1950 regulation 83 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 83 page for its amendments.
| Reg. 83 MATERIALS OF CONSTRUCTION FORGED OR ROLLED PRESSURE PARTS OTHER THAN SEAMLESS DRUMS OF CARBON STEEL Tensile strength |
| (a) The tensile strength of the material shall conform to one of the following four grades:- (i) 37 to 45 kgf/mm2 (b) The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength. (c) The minimum values of the stress at proof limit 0.2% at elevated temperature Et of the material may be calculated by multiplying the minimum specified tensile strength at room temperature R20 by the value of the ratio Et/R20 given in the table under Regulation 16. (d) The breaking elongation in percentage shall not be less than
|
IBR 1950 regulation 260 as last published in the DPIIT web edition (archived 2022)
Unofficial archived copy, not verified; see the regulation 260 page for its amendments.
|
| ||||||
Reg. 260
(b) All-weld Metal
|
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.


Indian Boiler Regulations, 2026, reg. 60, Regulation 60, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.546–547. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.