BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Indian Boiler Regulations, 2026 · Chapter 2 · Materials of Construction

Regulation 49. Seamless Carbon, Alloy Steel and Nickel Alloy Pipes

Official text — not yet verifiedGazette 1 Oct 2026 · printed pp. 530–537TableFormula / symbolsLong provision

Not yet checked against the official Gazette; verify before relying on it.

Reproduced from the Gazette of India · verification status above

49.Seamless Carbon, Alloy Steel and Nickel Alloy Pipes.– (1)This regulation shall apply on hot finished and cold drawn seamless carbon, alloy steel and Nickel alloy pipes for high temperature service and the pipes shall conform in all respects with the requirements under this regulation in addition to the requirements specified in regulation 30.

(2)For design metal temperatures Table 2/1 of regulation 30 shall be considered.

(3)(a)The pipes shall be seamless and manufactured from fully killed steel produced by an open hearth or electric process or any of the oxygen processes.

(b)The steel shall conform to the following limits of chemical composition, namely:–

Table 2/21: Chemical Composition (%)

Serial No.GradeChemical composition %
Carbon (C)Manganese( Mn)Silicon(Si)Sulphur( S)Phosphorus( P)Chromium( Cr)Molybdenum (Mo)Vanadium (V)Nickel (Ni)Copper (Cu)Other Elements
(1)(2)(3)(4)(5)(6)(7)(8)(9)(10)(11)(12)(13)
1.SA 106
Gr A
0.25*
Max
0.27
0.93
0.10M
in
0.035
Max
0.035
Max
0.40*
* Max
0.15*
*Max
0.08*
* Max
0.40*
* Max
0.40*
*
Max
2.SA 106
Gr B
0.30*
Min
0.29
1.06
0.10M
in
0.035
Max
0.035
Max
0.40*
* Max
0.15*
* Max
0.08*
* Max
0.40*
*Max
0.40*
*
Max
3.SA 106
Gr C
0.35*
Max
0.29
1.06
0.10M
in
0..035
Max
0.035
Max
0.40*
*Max
0.15*
*Max
0.08*
*max
0.40*
*Max
0.40*
*
Max
4.SA 335
Gr P1
0.10
0.20
0.30
0.80
0.10
0.50
0.025
max
0.025
max
----0.44
0.65
-------------
5.SA 335
Gr P2
0.10
0.20
0.30
0.61
0.10
0.30
0.025
max
0.025
max
0.50
0.81
0.44
0.65
-------------
6.SA 335
Gr P5
0.15
max
0.30
0.60
0.50
max
0.025
max
0.025
max
4.00
6.00
o.45
0.65
-------------
7.SA 335
Gr P9
0.15
max
0.30
0.60
0.25
1.00
0.025
max
0.025
max
8.00
10.0
0.90
1.10
-------------
8.SA 335
Gr P11
0.05
0.15
0.30
0.60
0.50
1.00
0.025
max
0.025
max
1.00
1.50
0.44
0.65
-------------
9.SA 335
Gr P12
0.05
0.15
0.30
0.61
0.50
max
0.025
max
0.025
max
0.80
1.25
0.44
0.65
-------------
10.SA 335
Gr P22
0.05
0.15
0.30
0.60
0.50
max
0.025
max
0.025
max
1.90
2.60
0.87
1.13
-------------
11.SA 335
Gr P91
0.08
0.12
0.30
0.60
0.20
0.50
0.010
max
0.020
max
8.00
9.50
0.85
1.05
0.18
0.25
0.40
max.
Cb=0.06 -
0.10
N=0.030 -
0.70
Al=0.02 max.
Ti=0.01 max.
Zr=0.01 max.
12.X20Cr
MoV121
0.17
0.23
1.00
max
0.50
max
0.03
max
0.030
max
10.0
12.5
0.80
1.20
0.25
0.35
0.30
0.80
----
13.SB 167
N06617
0.05
0.15
1.0
max
1.0
max
0.015
max
-20.02
4.0
8.0
10.0
-44.5
min
0.5
max
Co:10.0-15.0;
Fe:3.0 max;
Al: 0.8-1.5;
Ti:0.6 max;
B:0.006 max

Table structure read from the Gazette PDF, page 531. Verification status as for the text above.

* For each reduction of 0.01% below the specified carbon maximum, an increase of 0.06% manganese above the

specified maximum will be permitted up to a maximum of 1.35%.

Show original extracted text (diagnostic, not authoritative)
Serial No. Grade                                     Chemical composition %

                        Carbo Mang Silico Sulphur( Phosp Chro Molyb Vanad Nickel Coppe         Other

                        n (C)  anese(  n(Si)  S)     horus( mium( denum ium (Ni)        r      Elements
                               Mn)
                                                     P) Cr) (Mo) (V) (Cu)

(1)  (2)                (3)    (4)     (5)    (6)    (7)  (8)            (9)   (10) (11) (12)  (13)

1.   SA 106 0.25* 0.27 0.10M 0.035 0.035 0.40* 0.15* 0.08* 0.40* 0.40*

     Gr A               Max 0.93       in     Max    Max * Max *Max * Max * Max         *

                                                                                        Max

2.   SA 106 0.30* 0.29 0.10M 0.035 0.035 0.40* 0.15* 0.08* 0.40* 0.40*

     Gr B               Min 1.06       in     Max    Max * Max * Max * Max *Max         *

                                                                                        Max

3.   SA 106 0.35* 0.29 0.10M 0..035 0.035 0.40* 0.15* 0.08* 0.40* 0.40*

     Gr C               Max 1.06       in     Max    Max *Max *Max *max *Max            *

                                                                                        Max

4.   SA 335 0.10 0.30 0.10 0.025 0.025 ---- 0.44 ----                             ----         -----

     Gr P1              0.20 0.80 0.50        max    max                 0.65

5.   SA 335 0.10 0.30 0.10 0.025 0.025 0.50 0.44 ----                             ----         -----

     Gr P2              0.20 0.61 0.30        max    max 0.81 0.65

6.   SA 335 0.15 0.30 0.50 0.025 0.025 4.00 o.45 ----                             ----         -----

     Gr P5              max 0.60 max          max    max 6.00 0.65

7.   SA 335 0.15 0.30 0.25 0.025 0.025 8.00 0.90 ----                             ----         -----

     Gr P9              max 0.60 1.00         max    max 10.0 1.10

8.   SA 335 0.05 0.30 0.50 0.025 0.025 1.00 0.44 ----                             ----         -----

     Gr P11 0.15 0.60 1.00                    max    max 1.50 0.65

9.   SA 335 0.05 0.30 0.50 0.025 0.025 0.80 0.44 ----                             ----         -----

     Gr P12 0.15 0.61 max                     max    max 1.25 0.65

10.  SA 335 0.05 0.30 0.50 0.025 0.025 1.90 0.87 ----                             ----         -----

     Gr P22 0.15 0.60 max                     max    max 2.60 1.13

11.  SA 335 0.08 0.30 0.20 0.010 0.020 8.00 0.85 0.18 0.40                                     Cb=0.06 -
                                                                                                  0.10
     Gr P91 0.12 0.60 0.50                    max    max 9.50 1.05 0.25 max.
                                                                                               N=0.030 -

                                                                                                    0.70
                                                                                               Al=0.02 max.
                                                                                               Ti=0.01 max.
                                                                                               Zr=0.01 max.

12.  X20Cr              0.17 1.00 0.50        0.03 0.030 10.0 0.80 0.25 0.30                   ----

     MoV121 0.23 max max                      max    max 12.5 1.20 0.35 0.80

13.  SB 167 0.05 1.0                   1.0    0.015  -    20.02 8.0            -  44.5 0.5 Co:10.0-15.0;

     N06617 0.15 max max                      max         4.0 10.0                min max Fe:3.0 max;
                                                                                                        Al: 0.8-1.5;

                                                                                               Ti:0.6 max;
                                                                                               B:0.006 max

     * For each reduction of 0.01% below the specified carbon maximum, an increase of 0.06% manganese above the

     specified maximum will be permitted up to a maximum of 1.35%.

     ** Cr + Cu + Mo + Ni + V < 1.0 %

(4)(a)(i) Carbon Steel hot finished pipes need not be heat treated.

(ii)Cold drawn pipes shall be given a sub-critical anneal, a full anneal, or a normalising heat treatment after the final cold finishing process.

(b)(i)Pipes of grades P1, P2, P5, P9, P11, P12, and P22 except P91, X20CrMoV121 and N06617 shall be reheated and furnished in full annealed, isothermal annealed or normalised and tempered condition.

(ii)If furnished in the normalised and tempered condition, the minimum tempering temperature for grade P1, P2, P11 and P12 shall be 650°C and the minimum tempering temperature for grades P5, P9 and P22 shall be 675°C.

(c)Pipes of grades P1, P2 and P12 either hot finished or cold drawn may be given a final heat treatment at 650°C to 705°C, instead of heat treatment specified in clause (b) above at the option of the manufacturer.

(d)Grades P91 shall be normalised at 1040°C minimum and tempered at 730°C minimum as a final heat treatment.

(e)Grades X20CrMoV121 shall be normalised at 1020°C - 1070°C and tempered at 730°C - 780°C for a period of one hour minimum.

(f)Grade N06617 shall be solution annealed at 1150°C to 1230°C and quenched in water or rapidly cooled by other means.

(5)(a) (i)The pipes shall be finished, cleaned free from harmful defects.

(ii)They shall be reasonably straight, smooth, cylindrical and subject to the tolerance specified in this sub-regulation. Pipes manufacturer shall explore a sufficient number of visual inspections to provide reasonable assurance that they have been properly evaluated.

(b)Permissible variations in outside diameter shall be as follows:-

Table 2/22: Carbon Steel Hot finished and cold finished seamless pipes

Original extracted text of the table above, continued (diagnostic)
Serial No.  Outside diameter (mm)                          Permissible variations (mm)

      (1)                                Over                Under

1. (4)

Original extracted text of the table above, continued (diagnostic)
2.                (2)               (3)
3.
Serial No.Outside diameter (mm)Permissible variations (mm)
OverUnder
(1)(2)(3)(4)
1.10.3 to 48.3 incl.,0.400.40
2.Over 48.3 to 114.3 incl.,0..800.80
3.Over 114.3 to 219.1 incl.,1.600.80
4.Over 219.1 to 457.0 incl.,2.400.80
5.Over 457.0 to 660.0 incl.,3.200.80
6.Over 660.0 to 864.0 incl.,4.000.80
7.Over 864.0 to 1219.0 incl.,4.800.80

Table structure read from the Gazette PDF, page 532. Verification status as for the text above.

Table 2/23: For all grades of alloy steel except X20CrMoV121 and N06617

Serial No. Hot finished and Cold finished seamless pipes

Show original extracted text (diagnostic, not authoritative)
     4.     10.3 to 48.3 incl.,          0.40                0.40
     5.
     6.     Over 48.3 to 114.3 incl.,    0..80               0.80
     7.
            Over 114.3 to 219.1 incl.,   1.60                0.80

            Over 219.1 to 457.0 incl.,   2.40                0.80

            Over 457.0 to 660.0 incl.,   3.20                0.80

            Over 660.0 to 864.0 incl.,   4.00                0.80

            Over 864.0 to 1219.0 incl.,  4.80                0.80

            Table 2/23: For all grades of alloy steel except X20CrMoV121 and N06617

Serial No.  Hot finished and Cold finished seamless pipes

      (1)   Outside diameter (mm)                          Permissible variations (mm)
     1.
     2.                                         Over         Under
Original extracted text of the table above, continued (diagnostic)
3.
4.                (2)                      (3)                (4)
5.
       10.3 to 48.3 incl.                  0.40         0.40

       Over 48.3 to 114.3 incl.            0.80         0.80

       Over 114.3 to 219.1 incl.           1.60         0.80

       Over 219.1 to 300 incl.             2.40         0.80

       Over 300.                           1%                 1%

Table 2/24: For Grade X20CrMoV121

Serial No. Outside diameter (mm) Permissible variations (mm)

(1)Over Under

(4)

(2)(3)

Serial No.Outside diameter (mm)Permissible variations (mm)
OverUnder
(1)(2)(3)(4)
1.100 and under0.75%0.75%
2.Over 100 to 320 incl.0.90%0.90%
3.Over 3201.00%1.00%

Table structure read from the Gazette PDF, page 533. Verification status as for the text above.

Table 2/25: For Grade N06617

Serial No.Outside diameter (mm)Permissible Variation (mm)
OverUnder
(1)(2)(3)(4)
1.Seamless Cold-worked pipes
2.Over 10 and less than 160.130.13
3.16 - 380.190.19
4.Over 38 - 760.250.25
5.Over 76 to 1140.380.38
6.Over 114 to 1520.510.51
7.Over 152 to 1680.640.64
8.Over 168 to 2190.790.79
9.Hot finished pipes
10.64 to 1140.790.79
11.Over 114 to 1651.21.2
12.Over 165 to 2351.61.6

Table structure read from the Gazette PDF, page 533. Verification status as for the text above.

(c) Permissible variation in wall thickness shall be as follows:-:

Table 2/26: For grade X20CrMoV121

Show original extracted text (diagnostic, not authoritative)
    1.      100 and under               0.75%                             0.75%

    2.      Over 100 to 320 incl.       0.90%                             0.90%

    3.      Over 320                    1.00%                             1.00%

                                      Table 2/25: For Grade N06617

Serial No.  Outside diameter (mm)                                   Permissible Variation (mm)

                                                                    Over         Under

(1)                             (2)                                 (3)          (4)

1.          Seamless Cold-worked pipes

2.          Over 10 and less than 16                                0.13         0.13

3.          16 - 38                                                 0.19         0.19

4.          Over 38 - 76                                            0.25         0.25

5.          Over 76 to 114                                          0.38         0.38

6.          Over 114 to 152                                         0.51         0.51

7.          Over 152 to 168                                         0.64         0.64

8.          Over 168 to 219                                         0.79         0.79

9.          Hot finished pipes

10.         64 to 114                                               0.79         0.79

11.         Over 114 to 165                                         1.2          1.2

12.         Over 165 to 235                                         1.6          1.6

(c) Permissible variation in wall thickness shall be as follows:-:


                                Table 2/26: For grade X20CrMoV121

     Serial No.  Outside diameter (mm)                             Permissible variation %

(1)Over Under

Original extracted text of the table above, continued (diagnostic)
1.
2.                      (2)                              (3)   (4)
3.
Serial No.Outside diameter (mm)Permissible variation %
OverUnder
(1)(2)(3)(4)
1.100 and under12.510
2.Over 100 to 320 incl.12.512.5
3.Over 32015.012.5

Table structure read from the Gazette PDF, page 534. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
100 and under                                     12.5  10

Over 100 to 320 incl.                             12.5  12.5

Over 320                                          15.0  12.5

Table 2/27: For grade N06617

Serial No.Outside Diameter of pipe (mm)Permissible variation in Length (mm)
OverUnder
(1)(2)(3)(4)
1.Under 50.83.20
2.50.8 and over4.80

Table structure read from the Gazette PDF, page 535. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
Serial No.            Outside diameter (mm)                   Permissible Variation (mm)

                                                              Over  Under

    (1)                          (2)                          (3)   (4)

1. Seamless Cold-worked pipes

Original extracted text of the table above, continued (diagnostic)
2.          Over 10 and less than 16                          15.0  15.0

3.          16 - 38                                           10.0  10.0

4.          Over 38 - 76                                      10.0  10.0

5.          Over 76 to 114                                    10.0  10.0

6.          Over 114 to 152                                   12.5  12.5

7.          Over 152 to 168                                   12.5  12.5

8.          Over 168 to 219                                   12.5  12.5

9. Hot finished pipes

Original extracted text of the table above, continued (diagnostic)
10.         64 to 114                                         16.0  12.5

11.         Over 114 to 165                                   16.0  12.5

12.         Over 165 to 235                                   16.0  12.5

Note: For all grades, except X20CrMoV121 and N06617, the minimum wall thickness at any point shall not be more than 12.5% under the nominal wall thickness specified.

(d)Seamless Hot finished and Cold finished pipes can be ordered in specified length or in random length. If ordered in specified length, the tolerances shall be as follows:

Original extracted text of the table above, continued (diagnostic)
Serial No.         Grade                          Table 2/28     Permissible variation in (mm)
Serial No.GradeLength (m)Permissible variation in (mm)
OverUnder
(1)(2)(3)(4)(5)
1.All grades except
X20CrMoV121
and
N06617
All length60
2.For grade
X20CrMoV121
6 and under100
3.Over 6 to 12
incl.
150

Table structure read from the Gazette PDF, page 535. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
    (1)                                   Length (m)
                           (2)                              Over                  Under
1.            All grades except                (3)
              X20CrMoV121 and              All length          (4)                  (5)
2.            N06617
3.                                        6 and under          6                    0
              For grade                   Over 6 to 12
              X20CrMoV121                                      10                   0
Original extracted text of the table above, continued (diagnostic)
incl.
                15                   0

Table 2/29: For grade N06617

Original extracted text of the table above, continued (diagnostic)
Serial No.         Outside  Diameter  of pipe               Permissible variation in Length (mm)

(mm)(2)

Original extracted text of the table above, continued (diagnostic)
    (1)                                      Over                            Under
1.
2.                                                     (3)                   (4)

              Under 50.8                     3.2                             0

              50.8 and over                  4.8                             0

(6)(a)Test specimen required for flattening and expanding or flaring test specified in sub-regulations herein below shall be taken from ends of finished pipes prior to upsetting, swaging, expanding or any other forming operations or being cut to length and they shall be smooth on ends and free from burrs and flaws.

(b)If desirable and practicable, tensile test may be carried out on full section of the pipe up to the capacity of the testing machine and for large size pipes, the tensile test specimen shall consist of strip cut longitudinally from the pipe and which is not straightened within the gauge length and further heat treated.

(c)If any test specimen shows flaws or defective machining it may be discarded and another specimen substituted.

(d)All specimens shall be tested at room temperature.

(7)The tests specified in sub-regulations below shall be made on minimum 2 pipes for first 100 pipes and 1 per 100 or part thereof for pipes over 100 numbers from each lot. Lot applies to all pipes of same nominal size and wall thickness of same heat and heat treatment.

(8)(a)The tensile test may be carried out on the test pieces cut out from the pipe in the longitudinal direction which shall not be further heat treated nor straightened within the gauge length. As an alternative, pipes may be tested on full cross section.

(b)Test pieces cut from the ends of the selected pipes shall comply with the requirements specified in this sub-regulation.

Serial No.GradeYield Strength
MPa (kg/mm2)
min
Tensile Strength
MPa (kg/mm2)
min
%Elongation
on G.L.= 50 mm min *
for full tube testing
(1)(2)(3)(4)(5)
1.SA 106 Gr A205 (21.1)330 (33.1)35
2.SA 106 Gr B240 (24.7)415 (42.2)30
3.SA 106 Gr C275 (28.2)485 (49.3)30

Table structure read from the Gazette PDF, page 535. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
Serial No.         Grade                        Table 2/30  Tensile Strength            %Elongation
    (1)             (2)           Yield Strength            MPa (kg/mm2)          on G.L.= 50 mm min *
                                  MPa (kg/mm2)
                                                                   min              for full tube testing
                                        min                         (4)                       (5)
                                         (3)                                                  35

1.            SA 106 Gr A             205 (21.1)                 330 (33.1)                   30

2.            SA 106 Gr B             240 (24.7)                 415 (42.2)                   30

3.            SA 106 Gr C             275 (28.2)                 485 (49.3)

*The tensile test specimen shall be as per the relevant material specifications.

Note: For longitudinal strip test, the minimum required elongation shall be determined by the following equation:

e = 1940 (A 0.2/U0.9)

Where e = minimum elongation in 50.8 mm, % rounded to the nearest 0.5%.

A = cross sectional area of the tensile test specimen in mm2 based on specified outside diameter or nominal specimen width and specified wall thickness rounded to the nearest 6.45 mm2. If the area thus calculated is more than 484 mm2 then use area as 484 mm2. If the calculated area is less than 484 mm2 then use the actual area thus obtained.

U = specified tensile strength in MPa.

Table 2/31: Mechanical Property Requirements for Alloy Steels

Original extracted text of the table above, continued (diagnostic)
Serial No.  Grade          Yield Strength  Tensile Strength                       % elongation on GL=
    (1)      (2)           MPa (kg/mm2)    MPa (kg/mm2)                                50 mm min *

                                 min              min                                        (5)

(3)(4)

Serial No.GradeYield Strength
MPa (kg/mm2)
min
Tensile Strength
MPa (kg/mm2)
min
% elongation on GL=
50 mm min *
(1)(2)(3)(4)(5)
1.SA 335 Gr P1205 (21.1)380 (38.7)30
2.SA 335 Gr P2205 (21.1)380 (38.7)30
3.SA 335 Gr P5205 (21.1)415 (42.2)30
4.SA 335 Gr P9205 (21.1)415 (42.2)30
5.SA 335 Gr P11205 (21.1)415 (42.2)30
6.SA 335 Gr P12220 (22.5)415 (42.2)30
7.SA 335 Gr P22205 (21.1)415 (42.2)30
8.SA 335 Gr P91415 (42.2)585 (59.8)20
9.X20CrMoV121490 (50.0)690 (70.4)
840 (85.6)
17
10.SB 167 N06617240 (24.5)655 (66.8)35

Table structure read from the Gazette PDF, page 536. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
1.          SA 335 Gr P1   205 (21.1)                        380 (38.7)           30

2.          SA 335 Gr P2   205 (21.1)                        380 (38.7)           30

3.          SA 335 Gr P5   205 (21.1)                        415 (42.2)           30

4.          SA 335 Gr P9   205 (21.1)                        415 (42.2)           30

5.          SA 335 Gr P11  205 (21.1)                        415 (42.2)           30

6.          SA 335 Gr P12  220 (22.5)                        415 (42.2)           30

7.          SA 335 Gr P22  205 (21.1)                        415 (42.2)           30

8.          SA 335 Gr P91  415 (42.2)                        585 (59.8)           20

9.          X20CrMoV121    490 (50.0)                        690 (70.4)           17

                                                             840 (85.6)

10. SB 167 N06617          240 (24.5)                        655 (66.8)           35

*The tensile test specimen shall be as per the relevant material specifications.

(9)For pipes of outside diameter 60.3 millimetre(mm) and under, a bend test shall be conducted. A sufficient length of pipe shall stand being bent cold through 90° around a cylindrical mandrel, the diameter of which is 12 times the nominal diameter of the pipe, without developing cracks.

Provided that bend test shall be required for grade N06617.

(10)(a) For pipes of outside diameter over 60.3 mm, a flattening test shall be conducted and a section of the pipe not less than 63 mm in length shall be flattened cold between two parallel flat surfaces to a distance between the plates (H) as calculated by the formula given below, without showing any sign of a crack or flaw:

Original extracted text of the table above, continued (diagnostic)
           (1 + e) t
H = -----------
           e + t/D

where, t = specified thickness of pipe (mm)
D = specified outside diameter of the pipe (mm)
e = a constant, as given below
e = 0.07 for Carbon steel with maximum specified carbon above 0.18% e = 0.09 for Carbon steel with maximum specified carbon 0.18% or less. e = 0.08 for alloy steel

(b)For pipe whose diameter equals or exceeds 254 mm, a bend test may be conducted instead of the flattening test. The bend test specimens shall be bent at room temperature through 180° without cracking on the outside of the bent portion. The inside diameter of the bend shall be 25 mm. Substitution of the bend test for the flattening test shall be subject to the approval of the purchaser.

(c)For pipe whose diameter exceeds 635 millimetre(mm) and whose diameter to wall thickness ratio is

7.0 or less, the bend test described in sub-regulation (9) shall be conducted instead of the flattening test.

Provided that flattening test shall be required for grade N06617.

(11)(a) If any one or more tests specified in these regulations fail, two further tests of the same kind may be made on two other pipes of the same batch and if any of these tests fails, the batch of the pipes represented may be given a further heat treatment and entire set of tests shall be repeated.

(b)If the repeat tests are satisfactory the pipes shall be accepted and in case of any failure in the tests, the entire batch of the pipes shall be rejected.

(12)(a) Each pipe shall be tested by the manufacturer and shall withstand a hydraulic pressure to one and half time the design pressure, but not greater than pressure calculated by the formula given below and in the absence of working pressure indicated in the Test Certificate then the test pressure indicated in the Test Certificate divided by 1.5 shall be the maximum working pressure: P = 2St/D

Where, P = test pressure
D = specified outside diameter of the pipe
t = specified wall thickness of the pipe
S = stress which shall be taken as 40% of the minimum tensile strength at room temperature.

(b)Despite anything contained in the clause (a) above, the hydraulic test at the maker's works may be dispensed with, provided that the pipes are subject to non-destructive testing by an appropriate method like Ultrasonic or Eddy Current or Stray flux testing.

Parts of this extracted text look garbled; read the Gazette page before using any value.

Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.

Referenced provisions

Reg. 30

Independent explanation — not the law · draft · engineer review in progress

In short

Regulation 49 sets the requirements for hot finished and cold drawn seamless pipes of carbon, alloy steel and nickel alloy for high temperature service. These apply in addition to regulation 30, and design metal temperatures follow its Table 2/1.

Key points

  • (3) Pipes must be seamless, from fully killed steel made by open hearth, electric or oxygen process, with chemistry per Table 2/21. For the starred carbon steel grades, each 0.01% reduction below the carbon maximum permits a 0.06% increase in manganese above its maximum, up to 1.35%.
  • (4) Heat treatment: hot finished carbon steel pipes need none; cold drawn pipes get a sub-critical anneal, full anneal or normalising. Grades P1 to P22 are supplied annealed or normalised and tempered (minimum tempering 650°C for P1, P2, P11 and P12; 675°C for P5, P9 and P22). P91 is normalised at 1040°C minimum and tempered at 730°C minimum. Separate treatments are given for X20CrMoV121 and N06617.
  • (5) Pipes must be free from harmful defects and reasonably straight, smooth and cylindrical. Tables 2/22 to 2/29 give tolerances on outside diameter, wall thickness and specified length. Except for X20CrMoV121 and N06617, wall thickness may be no more than 12.5% under nominal at any point.
  • (6)–(7) Specimens come from finished pipe ends before forming. Test at least 2 pipes for the first 100, and 1 per 100 or part thereof beyond, from each lot of the same nominal size, wall thickness, heat and heat treatment.
  • (8) Tensile properties follow Table 2/30 (carbon steel) and Table 2/31 (alloy steels). For longitudinal strip tests, minimum elongation is found from the equation given, with a cap on the area used.
  • (9) Pipes of 60.3 mm outside diameter and under get a cold bend test through 90° around a mandrel of 12 times the nominal diameter.
  • (10) Pipes over 60.3 mm get a flattening test on a section at least 63 mm long, using the H formula with constant e for carbon or alloy steel. From 254 mm, a 180° bend test may replace it with the purchaser's approval. Over 635 mm with a diameter to wall thickness ratio of 7.0 or less, the bend test in (9) replaces it.
  • (12)(a) Each pipe withstands a hydraulic test of one and half times the design pressure, but not above P = 2St/D, with S at 40% of minimum room-temperature tensile strength. Where no working pressure is shown on the Test Certificate, the maximum working pressure is the test pressure divided by 1.5.

Watch out

  • (11) If a test fails, two more tests are made on two other pipes. If either fails, the batch may be re-heat treated and all tests repeated; any further failure rejects the entire batch.
  • (12)(b) The works hydraulic test may be dispensed with if pipes get suitable NDT, such as Ultrasonic, Eddy Current or Stray flux testing.
  • The provisos in (9) and (10) about grade N06617, and several tables, may not have extracted cleanly. Check the Gazette page for the exact wording and values.

Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.

Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).

Orientation hints (unverified)

These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.

No candidate heading found in the historical print edition.

Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Instrument
Indian Boiler Regulations, 2026 (made by the Central Boilers Board under s.40 of the Boilers Act, 2025)
Notification
F.No. P-30014/3/2021-Boiler dated 7 Aug 2026
Published
Gazette of India, Extraordinary, Part III Sec. 4, No. 596, 1 Oct 2026 (CG-DL-E-06102026-276813)
In force
1 Oct 2026 (reg. 1(3): date of publication in the Official Gazette)
Printed Gazette page
530–537
PDF page index
530–537 · open official e-Gazette PDF
Extraction
pdftotext layout mode, sequential regulation detector · text hash b4afc4c934f3d212
Verification
Official text — not yet verified
Amendments checked
None known after 1 Oct 2026 as of build date (not a guarantee). Amendment log
How to cite

Indian Boiler Regulations, 2026, reg. 49, Regulation 49, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.530–537. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).

The citation refers to the government publication. Cite the Gazette, not this website.

Help improve this page

Engineers like you keep IBRsource accurate. Every checked correction or tip helps the next reader.