Official text — not yet verifiedGazette 1 Oct 2026 · printed p. 520Formula / symbols

Not yet checked against the official Gazette; verify before relying on it.

Reproduced from the Gazette of India · verification status above

39. Bend tests in case of cold bends,─(1)Test pieces shall be sheared lengthwise or crosswise from plates or bars, and shall not be less than 38 millimeter(mm) wide, but for small bars the whole section may be used.

(2)(a)In all cold bend tests, on samples 13 millimeter (mm) in thickness and above, the rough edge or bur caused by shearing may be removed by filling or grinding and samples 25 millimeter(mm) in thickness and above may have the edges machined, but the test pieces shall receive no other preparation.

(b)The test pieces shall not be annealed unless the material from which they are cut is similarly annealed and in such case the test piece shall be similarly treated with the material before testing.

(3)For bend test of plates of all grades of steel, the test piece shall withstand, without fracture, being bent cold through 180° around a mandrel, the radius of which shall have a relationship to the plate thickness as given below:─

Serial No.Tensile strengthMandrel Radius
(1)(2)(3)
1.36 - 49 kg/mm21 T*
2.41 - 57 kg/mm21 T
3.45 - 64 kg/mm21.5 T

Table structure read from the Gazette PDF, page 520. Verification status as for the text above.

Show original extracted text (diagnostic, not authoritative)
Serial No.           Tensile strength        Mandrel Radius
     (1)                    (2)                     (3)
         1.                                        1 T*
         2.          36 - 49 kg/mm2                 1 T
         3.          41 - 57 kg/mm2                1.5 T
                     45 - 64 kg/mm2

*Where, T = Plate thickness

(4)For small sectional material the bend tests may be made from the flattened bar.

(5)Bend tests may be made either by pressure or by blows.

Parts of this extracted text look garbled; read the Gazette page before using any value.

Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.

Independent explanation — not the law · draft · engineer review in progress

In short

Regulation 39 sets how cold bend test pieces are prepared and what they must withstand.

Key points

  • (1) Test pieces are sheared lengthwise or crosswise from plates or bars and are at least 38 mm wide. For small bars the whole section may be used.
  • (2)(a) For samples 13 mm thick and above, the shearing burr may be removed by filing or grinding. Samples 25 mm thick and above may have the edges machined. No other preparation is allowed.
  • (2)(b) Test pieces are annealed only if the material they come from is similarly annealed, and then they are treated the same way before testing.
  • (3) For plates of all steel grades, the test piece must bend cold through 180° around a mandrel without fracture. The mandrel radius is a multiple of the plate thickness T and depends on the tensile strength range. The table is misaligned in the extracted text, so check the Gazette page for the exact values.
  • (4)–(5) Small sections may be tested from the flattened bar. Bends may be made by pressure or by blows.

Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.

Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).

Orientation hints (unverified)

These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.

Historical 1950-edition reg.Heading as OCR'dHeading similaritySource image
19Bend Tests100%Chapter II (DPIIT scan), image 2
84Bend Tests100%Chapter II (DPIIT scan), image 16
262Bend Tests100%Chapter V (DPIIT scan), image 7

Amendment history of the candidate IBR 1950 regulations: Reg. 19 (1 amendment)

IBR 1950 regulation 19 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 19 page for its amendments.

Reg. 19
MATERIALS OF CONSTRUCTION

STEEL PLATES, RIVETS, SECTION AND BARS IN CARBON STEEL

Bend Tests

Cold Bends.-(a) Test pieces shall be sheared lengthwise or crosswise from plates or bars, and shall not be less than 1½ inches wide, but for small bars the whole section may be used. For rivet bars bend tests are not required.

b) In all cold bend tests, on samples 0.5 inch in thickness and above, the rough edge or arris caused by shearing may be removed by filing or grinding, and samples 1 inch in thickness and above may have the edges machined, but the test pieces shall receive no other preparation. The test pieces shall not be annealed unless the material from which they are cut is similarly annealed in which case the test piece shall be similarly and simultaneously treated with the material before testing. 

(c) (i) For bend test of plates of all grades of steel, the test piece shall withstands, without fracture, being bent cold through 180o around a mandrel, the radius of which shall have a relationship to the plate thickness as given below:

      Tensile strength                          Mandrel Radius

      36 - 49 kg./mm2                              1 T

      41 - 57 kg./mm2                              1 T

      45 - 64 kg./mm2                            1.5 T

where T = Plate thickness  

(ii) For cold bend test of sections and bars, the test piece shall withstand, without fracture, being doubled over until the internal radius is equal to that shown in Table under regulation 16 and the limbs are parallel.

(d) For small sectional material these bend tests may be made from the flattened bar.

(e) Bend tests may be made either by pressure or by blows.

IBR 1950 regulation 84 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 84 page for its amendments.

Reg. 84
MATERIALS OF CONSTRUCTION

FORGED OR ROLLED PRESSURE PARTS OTHER THAN SEAMLESS DRUMS OF CARBON STEEL

Bend Tests

(a) Bend test pieces shall be of rectangular cross section machined to a finished size of 1 inch wide by ¾ inch thick. In the case of headers, bend test pieces may be cut transversely 1½ T wide by T thick where T is the thickness of the header. The edges shall be rounded to a radius of 1/16 inch. The test pieces shall be bent over the thinner section.

(b) Test pieces shall be bent when cold through an angle of 180° without fracture, the internal radius of the bend being not greater than that specified in table below for the 1 inch wide by ¾ inch thick test piece and not more than 1½ T for the full thickness test piece:

Ultimate tensile stress

Internal radius of bend

Tons/sq. inch

Inch

Upto 32 1/4
Above 32 and upto 36 3/8
Above 36 and upto 38 5/8

Bend tests may be made by pressure or by blows.
IBR 1950 regulation 262 as last published in the DPIIT web edition (archived 2022)

Unofficial archived copy, not verified; see the regulation 262 page for its amendments.


Reg. 261
, Reg. 262, Reg. 263

Bend Test Pieces

a)

One for direct and one for reverse bending shall be taken transversely to the weld and where the thickness of the plate permits, one should be above the other. The specimens shall be rectangular in section so as to have width equal to one and half times the thickness of the specimen but not less than 30 mm. The surface of the specimens shall be machined just to remove the surface irregularities of the plate and the weld. The corners of the specimens shall be rounded to a radius not exceeding 10% of the thickness of the specimen.
b)

Where plate thicknesses do not exceed, 1¼ in. the thickness of the specimen shall be equal to the full thickness of the test plate. Where the plate thickness exceeds 1¼ in. the specimen shall in all cases have a thickness of at least 1¼ in. The specimen to be tested with the outer surface of the weld in tension shall be prepared by cutting to waste the metal local to the inner surface of the weld so that the desired specimen thickness is obtained (see Fig.20, Specimen A). the specimen to be tested with the inner surface in tension shall be prepared by cutting to waste the metal local to the outer surface of the weld so that the desired specimen thickness is obtained (see Fig.20, Specimen B). Where the thickness of the plate permits, both specimens may be cut from the same piece of plate, the specimen being located in the plate one above the other (see Fig. 20, Specimen C).



Reg. 262

Bend Tests

The specimen shall be mounted in such a way that the axis of the former is in the middle of the weld, and on roller supports the faces of which are separated by a distance determined by the thickness of the specimen.

The test specimen shall be pushed through the supports by a former having a diameter also determined by the thickness of the specimen. The requirements of the Table below, relating to the thickness of the test specimen shall apply.

 Table: Bend Test Requirements

Specified minimum tensile strength of plate Diameter
of former
Free space between supports at the end of test
Below 44 kgf/mm² 2t 4.2t
From 44 to 54 kgf/mm² 3t 5.2t
Above 54 kgf/mm² 4t 6.2t

On completion of the test, no crack or defect on the outer surface of the specimen shall be greater than 1.5 mm measured across the specimen, or 3 mm measured along the specimen. Premature failure at the corner of the specimen shall not be considered as a cause for rejection.



Reg. 263

Notched-Bar Impact Tests

The notched bar impact test specimens are to be one of the two types and dimension shown in figure 21A and 21B. The notch shall be contained in the weld-metal at approximately the axis of the weld and the axis of the notch is to be perpendicular to the surface of the plate.

The test shall be carried out as follows:-
For the U-Notch specimen at a temperature of 20 ± 2°C.
For the V-Notch specimen at a temperature of 50 ± 2°C.
In the case of V-Notch specimen, the machining of the bottom of the notch shall be done very carefully.

The choice between U-notch and V-notch specimen shall be at the discretion of the Inspecting Authority. The minimum result to be obtained from the Impact test pieces shall be:

a) U-notch specimen 5.50 kgfm/cm²
b) V-notch specimen 3.46 kgfm/cm²

Note: Above values are equivalent to 2.76 kgfm divided by sectional area below the notch.

Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.

Instrument
Indian Boiler Regulations, 2026 (made by the Central Boilers Board under s.40 of the Boilers Act, 2025)
Notification
F.No. P-30014/3/2021-Boiler dated 7 Aug 2026
Published
Gazette of India, Extraordinary, Part III Sec. 4, No. 596, 1 Oct 2026 (CG-DL-E-06102026-276813)
In force
1 Oct 2026 (reg. 1(3): date of publication in the Official Gazette)
Printed Gazette page
520
PDF page index
520 · open official e-Gazette PDF
Extraction
pdftotext layout mode, sequential regulation detector · text hash 656e64365a5b4475
Verification
Official text — not yet verified
Amendments checked
None known after 1 Oct 2026 as of build date (not a guarantee). Amendment log
How to cite

Indian Boiler Regulations, 2026, reg. 39, Regulation 39, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.520. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).

The citation refers to the government publication. Cite the Gazette, not this website.

Help improve this page

Engineers like you keep IBRsource accurate. Every checked correction or tip helps the next reader.