Indian Boiler Regulations, 2026 · Chapter 2 · Materials of Construction
Regulation 75. Regulation 75
Not yet checked against the official Gazette; verify before relying on it.
75.(1) Initial tests of each brand of electrodes shall be carried out in accordance with these regulations and relevant AWS or SFA specification.
(2)(a) All weld metal tensile test specimens shall be prepared and tested in accordance with the method described in Appendix-C.
(b)The ultimate tensile stress, yield stress and elongation of each test specimen shall meet the relevant AWS or SFA specification.
(3)One fillet weld hot cracking test shall be carried out as specified in Appendix-C.
(4)(a)The electrodes shall be deemed to be satisfactory provided no hot cracking occurs under the conditions of test.
(b)Crater cracks may be neglected provided they do not run into the full section of the weld.
(5)One transverse tensile test shall be carried out for each welding position for which the electrode is recommended by the manufacturer except two tests shall be required for the flat position. The ultimate tensile stress shall meet the relevant AWS or SFA specification. The method of preparation of the test pieces is specified in Appendix-C.
(6)Two bend tests one with the face and the other with the root in tension shall be carried out for each welding position for which the electrode is recommended by the manufacturer, except that two in each shall be carried out for those intended for flat position only. The method of preparation and carrying out the test shall be in accordance with Appendix-C. The electrode shall be deemed to be satisfactory provided that on completion of the test, no crack or defect at the outer surface is greater than 3 mm measured across the specimen or 1.6 mm measured along its length. Premature failures at corners of the test specimen shall not be considered a cause for rejection. For nickel alloy electrodes three transverse side bend test shall be carried out as per the applicable AWS or SFA specification.
(7)Five impact test specimens are required for carbon steel and low alloy steel electrodes only. The size of the electrode shall be as per the relevant AWS or SFA specification. Charpy V notch testing shall be carried out as per the applicable AWS or SFA specification.
(8)Each classification of electrode shall be tested for the chemical analysis of undiluted weld metal as per the relevant AWS or SFA specification.
(9)(a) All weld test plate shall be radiographed to evaluate the usability of the electrode and the soundness of the weld deposits prior to taking up for other tests.
(b)For the purpose of radiography, the backing plate shall be removed and both the surfaces of the weld metal shall be machined or ground smooth and flush without reducing the thickness of the weld metal.
(c)Test procedure and acceptance norms shall be in accordance with the relevant AWS or SFA specification.
(d)A length of 25 mm from both the ends of the test plate shall be discarded and need not be considered in evaluation of the radiograph.
In short
Regulation 75 lists the initial tests for each brand of welding electrode, carried out under these regulations and the relevant AWS or SFA specification. Test methods are in Appendix-C.
Key points
- (2) All-weld-metal tensile tests: ultimate tensile stress, yield stress and elongation must meet the AWS or SFA specification.
- (3), (4) One fillet weld hot cracking test. The electrode passes if no hot cracking occurs. Crater cracks may be neglected if they do not run into the full section of the weld.
- (5) One transverse tensile test for each welding position the manufacturer recommends, but two for the flat position.
- (6) Two bend tests (face and root in tension) per recommended position. Pass if no crack or defect at the outer surface exceeds 3 mm across the specimen or 1.6 mm along its length. Premature failures at the corners do not count. Nickel alloy electrodes get three transverse side bend tests instead, as per AWS or SFA.
- (7) Five Charpy V-notch impact specimens, for carbon steel and low alloy steel electrodes only.
- (8) Chemical analysis of undiluted weld metal for each classification.
- (9) All weld test plates are radiographed before other tests, with the backing plate removed and both surfaces machined or ground flush without reducing weld thickness. 25 mm at each end of the plate is discarded from the evaluation.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
No candidate heading found in the historical print edition.
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.


Indian Boiler Regulations, 2026, reg. 75, Regulation 75, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.558–559. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.