Indian Boiler Regulations, 2026 · Chapter 2 · Materials of Construction
Regulation 58. Forgingsof carbon, alloy, stainless steel and nickel alloys
Not yet checked against the official Gazette; verify before relying on it.
58.Forgingsof carbon, alloy, stainless steel and nickel alloys.–(1) The steel used for the forgings shall be made by an Open Hearth or Electric or basic Oxygen process or by any other process which gives steel having equivalent properties.
(2)(a)The steel shall not contain more than 0.05 per cent of sulphur or of phosphorus.
(b)The steel shall comply with the chemical composition specified in the Table 2/35.
Table 2/35: Chemical composition (%)
| Serial No. | Grade | Carbon (C) | Manganese (Mn) | Phosphorus (P) | Sulphur(S) | Silicon(Si) | Chromium (Cr) | Nickel(Ni) | Molybdenum (Mo) | Vanadium(V) | Nitrogen (N) | Others |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| (1) | (2) | (3) | (4) | (5) | (6) | (7) | (8) | (9) | (10) | (11) | (12) | (13) |
| 1. | SA 266 Gr1 | 0.30 | 0.40–1.05 | 0.025 | 0.025 | 0.15–0.35 | - | - | - | - | - | - |
| 2. | SA 266 Gr2 | 0.30 | 0.40–1.05 | 0.025 | 0.025 | 0.15–0.35 | - | - | - | - | - | - |
| 3. | SA 266 Gr3 | 0.35 | 0.80–1.35 | 0.025 | 0.025 | 0.15–0.35 | - | - | - | - | - | - |
| 4. | SA 350 LF1-Note 4 | 0.30 | 0.60–1.35 | 0.035 | 0.040 | 0.15–0.30 | 0.30 | 0.40 | 0.12 | 0.08 | - | Nb-0.02 Cu-0.04 |
| 5. | SA 350 LF2-Note 4 | 0.30 | 0.60–1.35 | 0.035 | 0.040 | 0.15–0.30 | 0.30 | 0.40 | 0.12 | 0.08 | - | Nb-0.02 Cu-0.04 |
| 6. | SA 105 - Note 4 | 0.35 | 0.60–1.05 | 0.035 | 0.040 | 0.10–0.35 | 0.30 | 0.40 | 0.12 | 0.08 | - | Cu-0.4 |
| 7. | SA 182 F1 | 0.28 | 0.60–0.90 | 0.045 | 0.045 | 0.15–0.35 | - | - | 0.44–0.65 | - | - | - |
| 8. | SA 182 F2 | 0.05–0.21 | 0.30–0.80 | 0.040 | 0.040 | 0.10–0.60 | 0.50–0.81 | - | 0.44–0.65 | - | - | - |
| 9. | SA 182 F11 Cl 1 | 0.05–0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50–1.00 | 1.00–1.50 | - | 0.44–0.65 | - | - | - |
| 10. | SA 182 F11 Cl 2 | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.50–1.00 | 1.00–1.50 | - | 0.44–0.65 | - | - | - |
| 11. | SA 182 F11 Cl 3 | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.50–1.00 | 1.00–1.50 | - | 0.44–0.65 | - | - | - |
| 12. | SA 182 F12 Cl 1 | 0.05–0.15 | 0.30–0.60 | 0.045 | 0.045 | 0.50 | 0.80–1.25 | - | 0.44–0.65 | - | - | - |
| 13. | SA 182 F12 Cl 2 | 0.10–0.20 | 0.30–0.80 | 0.040 | 0.040 | 0.10–0.60 | 0.80–1.25 | - | 0.44–0.65 | - | - | - |
| 14. | SA 182 F22 Cl 1,3 | 0.05–0.15 | 0.30–0.60 | 0.040 | 0.040 | 0.50 | 2.00–2.50 | - | 0.87–1.13 | - | - | - |
| 15. | SA 182 F5 | 0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50 | 4.0–6.0 | 0.50 | 0.44–0.65 | - | - | - |
| 16. | SA 182 F9 | 0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50–1.00 | 8.0–10.0 | - | 0.90–1.10 | - | - | - |
| 17. | SA 182 F91 | 0.08–0.12 | 0.30–0.60 | 0.020 | 0.010 | 0.20–0.50 | 8.0–9.5 | 0.40 | 0.85–1.05 | 0.18–0.25 | 0.03–0.07 | Nb-0.06–0.10; Al 0.02 Ti 0.01; Zr 0.01 |
| 18. | SA 182 F304 | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 18.0–20.0 | 8.0-11.0 | - | - | 0.10 | - |
| 19. | SA 182 F304H | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 18.0–20.0 | 8.0–11.0 | - | - | - | - |
| 20. | SA 182 F304L | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 18.0–20.0 | 8.0–13.0 | - | - | 0.10 | - |
| 21. | SA 182 F316 | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 16.0-18.0 | 10.0-14.0 | 2.0-3.0 | - | 0.10 | - |
| 22. | SA 182 F316H | 0.04-0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 16.0-18.0 | 10.0-14.0 | 2.0-3.0 | - | - | - |
| 23. | SA 182 F316L | 0.030 | 2.00 | 0.045 | 0.030 | 1.00 | 16.0-18.0 | 10.0-15.0 | 2.0-3.0 | - | 0.10 | - |
| 24. | SA 182 F321 | 0.08 | 2.00 | 0.045 | 0.030 | 1.00 | 17.0-19.0 | 9.0-12.0 | - | - | - | J |
| 25. | SA 182 F321H | 0.04-0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 17.0-19.0 | 9.0-12.0 | - | - | - | K |
| 26. | SA 182 F347H | 0.04–0.10 | 2.00 | 0.045 | 0.030 | 1.00 | 17.0–20.0 | 9.0–13.0 | - | - | - | M |
| 27. | SA 234 WPB-Note 2 | 0.30 | 0.29–1.06 | 0.050 | 0.058 | 0.10 min | 0.40 | 0.40 | 0.15 | 0.08 | - | - |
| 28. | SA 234 WPC | 0.35 | 0.29–1.06 | 0.050 | 0.058 | 0.10 min | 0.40 | 0.40 | 0.15 | 0.08 | - | - |
| 29. | SA 234 WP11 Cl 1 | 0.05–0.15 | 0.30–0.60 | 0.030 | 0.030 | 0.50–1.00 | 1.00–1.50 | - | 0.44–0.65 | - | - | - |
| 30. | SA 234 WP12 Cl 1 | 0.05–0.20 | 0.30–0.80 | 0.045 | 0.045 | 0.60 | 0.80–1.25 | - | 0.44–0.65 | - | - | - |
| 31. | SA 234 WP22 Cl 1 | 0.05–0.15 | 0.30–0.60 | 0.040 | 0.040 | 0.50 | 1.90–2.60 | - | 0.87–1.13 | - | - | - |
| 32. | SA 234 WP5 Cl1 | 0.15 | 0.30–0.60 | 0.040 | 0.030 | 0.50 | 4.0–6.0 | - | 0.44–0.65 | - | - | - |
| 33. | SA 234 WP9 Cl1 | 0.15 | 0.30–0.60 | 0.030 | 0.030 | 1.00 | 8.0–10.0 | - | 0.90–1.10 | - | - | - |
| 34. | SA 234 WP91 | 0.08–0.12 | 0.30–0.60 | 0.020 | 0.010 | 0.20–0.50 | 8.0–9.5 | - | 0.85–1.05 | - | - | - |
| 35. | SA 336 F11 Cl 1 | 0.05–0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.50–1.00 | 1.00–1.50 | - | 0.44–0.65 | - | - | - |
| 36. | SA 336 F11 Cl 2,3 | 0.10–0.20 | 0.30–0.80 | 0.025 | 0.025 | 0.50–1.00 | 1.00–1.50 | - | 0.45–0.65 | - | - | - |
| 37. | SA 336 F12 | 0.10–0.20 | 0.30–0.80 | 0.025 | 0.025 | 0.10–0.60 | 0.80–1.10 | - | 0.45–0.65 | - | - | - |
| 38. | SA 336 F5 | 0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.50 | 4.0–6.0 | 0.50 | 0.45–0.65 | - | - | - |
| 39. | SA 336 F9 | 0.15 | 0.30–0.60 | 0.025 | 0.025 | 0.50–1.00 | 8.0–10.0 | - | 0.90–1.10 | - | - | - |
| 40. | SA 336 F91 | 0.08–0.12 | 0.30–0.60 | 0.025 | 0.025 | 0.20–0.50 | 8.0–9.5 | 0.40 | 0.85–1.05 | 0.18–0.25 | 0.03–0.07 | Nb-0.06–0.10; Al- 0.02 Ti-0.01; Zr-0.01 |
| 41. | SB 564 N06617 SB 166 N06617 | 0.05-0.15 | 1.0 | - | 0.015 | 1.0 | 20.0-24.0 | 44.5 min | 8.0-10.0 | - | - | Co:10.0-15.0; Fe:3.0; Al: 0.8-1.5; Cu:0.5; Ti:0.6; B:0.006 |
Table structure read from the Gazette PDF, pages 544, 545. Verification status as for the text above.
Note: 1. Maximum when single values specified
2. For SA 234 WPB, Fittings made from bar or plate may have 0.35 max carbon.
Show original extracted text (diagnostic, not authoritative)
Serial No. Grade Carbon Manganese Phosphorus Sulphur(S) Silicon(Si) Chromium Nickel(Ni) Molybdenum Vanadium(V) Nitrogen (N) Others
(C) (Mn) (P) (Mo)
(3) (4) (5) (Cr) (10) (11) (12) (13)
0.30 0.025 - - - -
(1) (2) 0.30 0.40–1.05 0.025 (6) (7) (8) (9) - - - -
0.35 0.40–1.05 0.025 - - - -
1. SA 266 Gr1 0.80–1.35 0.025 0.15–0.35 - -
0.30 0.035 Nb-0.02
2. SA 266 Gr2 0.60–1.35 0.025 0.15–0.35 - - Cu-0.04
0.30 Nb-0.02
3. SA 266 Gr3 0.025 0.15–0.35 - - Cu-0.04
0.35 Cu-0.4
4. SA 350 LF1-Note 4 0.28 0.040 0.15–0.30 0.30 0.40 0.12 0.08 -
0.05–0.21 -
5. SA 350 LF2-Note 4 0.05–0.15 0.60–1.35 0.035 0.040 0.15–0.30 0.30 0.40 0.12 0.08 - -
0.10–0.20 -
6. SA 105 - Note 4 0.10–0.20 0.60–1.05 0.035 0.040 0.10–0.35 0.30 0.40 0.12 0.08 - -
7. SA 182 F1 0.05–0.15 0.60–0.90 0.045 -
8. SA 182 F2 0.10–0.20 0.30–0.80 0.040 0.045 0.15–0.35 - - 0.44–0.65 - - -
9. SA 182 F11 Cl 1 0.05–0.15 0.30–0.60 0.030 -
10. SA 182 F11 Cl 2 0.15 0.30–0.80 0.040 0.040 0.10–0.60 0.50–0.81 - 0.44–0.65 - - -
11. SA 182 F11 Cl 3 0.15 0.30–0.80 0.040 -
12. SA 182 F12 Cl 1 0.30–0.60 0.045 0.030 0.50–1.00 1.00–1.50 - 0.44–0.65 - - -
13. SA 182 F12 Cl 2 0.08–0.12 0.30–0.80 0.040 Nb-0.06–0.10; Al
14. SA 182 F22 Cl 1,3 0.30–0.60 0.040 0.040 0.50–1.00 1.00–1.50 - 0.44–0.65 - - 0.02
15. SA 182 F5 0.08 0.30–0.60 0.030 Ti 0.01; Zr 0.01
16. SA 182 F9 0.04–0.10 0.30–0.60 0.030 0.040 0.50–1.00 1.00–1.50 - 0.44–0.65 - - -
17. -
0.030 0.045 0.50 0.80–1.25 - 0.44–0.65 - - -
SA 182 F91 0.08 -
0.04-0.10 0.040 0.10–0.60 0.80–1.25 - 0.44–0.65 - - -
0.030 -
0.08 0.040 0.50 2.00–2.50 - 0.87–1.13 - - J
0.04-0.10 K
0.030 0.50 4.0–6.0 0.50 0.44–0.65 - -
0.030 0.50–1.00 8.0–10.0 - 0.90–1.10 - -
0.30–0.60 0.020 0.010 0.20–0.50 8.0–9.5 0.40 0.85–1.05 0.18–0.25 0.03–0.07
18. SA 182 F304 2.00 0.045 0.030 1.00 18.0–20.0 8.0-11.0 - - 0.10
19. SA 182 F304H 0.030
20. SA 182 F304L 2.00 0.045 0.030 1.00 18.0–20.0 8.0–11.0 - - -
21. SA 182 F316 0.030
22. SA 182 F316H 2.00 0.045 0.030 1.00 18.0–20.0 8.0–13.0 - - 0.10
23. SA 182 F316L 0.030
24. SA 182 F321 2.00 0.045 0.030 1.00 16.0-18.0 10.0-14.0 2.0-3.0 - 0.10
25. SA 182 F321H 0.030
2.00 0.045 1.00 16.0-18.0 10.0-14.0 2.0-3.0 - -
2.00 0.045 1.00 16.0-18.0 10.0-15.0 2.0-3.0 - 0.10
2.00 0.045 1.00 17.0-19.0 9.0-12.0 - - -
2.00 0.045 1.00 17.0-19.0 9.0-12.0 - - -
26. SA 182 F347H 0.04–0.10 2.00 0.045 0.030 1.00 17.0–20.0 9.0–13.0 - - - M
27. SA 234 WPB-Note 2 0.30 0.29–1.06 0.050 0.058 0.10 min 0.40 0.40 0.15 0.08 - -
28. SA 234 WPC 0.35 0.29–1.06 0.050 0.058 0.10 min 0.40 0.40 0.15 0.08 - -
29. SA 234 WP11 Cl 1 0.05–0.15 0.30–0.60 0.030 0.030 0.50–1.00 1.00–1.50 - 0.44–0.65 - - -
30. SA 234 WP12 Cl 1 0.05–0.20 0.30–0.80 0.045 0.045 0.60 0.80–1.25 - 0.44–0.65 - - -
31. SA 234 WP22 Cl 1 0.05–0.15 0.30–0.60 0.040 0.040 0.50 1.90–2.60 - 0.87–1.13 - - -
32. SA 234 WP5 Cl1 0.15 0.30–0.60 0.040 0.030 0.50 4.0–6.0 - 0.44–0.65 - - -
33. SA 234 WP9 Cl1 0.15 0.30–0.60 0.030 0.030 1.00 8.0–10.0 - 0.90–1.10 - - -
34. SA 234 WP91 0.08–0.12 0.30–0.60 0.020 0.010 0.20–0.50 8.0–9.5 - 0.85–1.05 - - -
35. SA 336 F11 Cl 1 0.05–0.15 0.30–0.60 0.025 0.025 0.50–1.00 1.00–1.50 - 0.44–0.65 - - -
36. SA 336 F11 Cl 2,3 0.10–0.20 0.30–0.80 0.025 0.025 0.50–1.00 1.00–1.50 - 0.45–0.65 - - -
37. SA 336 F12 0.10–0.20 0.30–0.80 0.025 0.025 0.10–0.60 0.80–1.10 - 0.45–0.65 - - -
38. SA 336 F5 0.15 0.30–0.60 0.025 0.025 0.50 4.0–6.0 0.50 0.45–0.65 - - -
39. SA 336 F9 0.15 0.30–0.60 0.025 0.025 0.50–1.00 8.0–10.0 - 0.90–1.10 - - -
40. SA 336 F91 Nb-0.06–0.10; Al-
0.08–0.12 0.30–0.60 0.025 0.025 0.20–0.50 8.0–9.5 0.40 0.85–1.05 0.18–0.25 0.03–0.07 0.02
Ti-0.01; Zr-0.01
41. SB 564 N06617 0.05-0.15 1.0 - 0.015 1.0 20.0-24.0 44.5 min 8.0-10.0 - - Co:10.0-15.0; Fe:3.0;
SB 166 N06617 Al: 0.8-1.5; Cu:0.5;
Ti:0.6; B:0.006
Note: 1. Maximum when single values specified
2. For SA 234 WPB, Fittings made from bar or plate may have 0.35 max carbon.
3. For SA 234 WPB & SA 234 WPC Fittings:(i)The sum of copper, nickel, chromium, molybdenum and vanadium shall not exceed 1.00%.
(ii)Fittings made from forgings may have 0.35 max carbon and 0.35 max silicon with no minimum
(iii)For each reduction of 0.01 % below the specified carbon maximum, an increase of 0.06 % manganese above the specified maximum will be permitted, up to a maximum of 1.65 %.
4. For SA 350 LF1, LF2 & SA 105 Forgings
(i)The sum of chromium and molybdenum shall not exceed 0.32%.
(ii)The sum of copper, nickel, chromium, molybdenum and vanadium shall not exceed 1.00%.
5. J Grade F 321 shall have a titanium content of not less than five times the carbon content and not more than 0.70 %.
K Grade F 321H shall have a titanium content of not less than four times the carbon content and not more than 0.70 %.
M Grades F 347H shall have a columbium content of not less than eight times the carbon content and not more than 1.10 %.
(3)Heat treatment shall be as per relevant material specifications.
(4)Where not machined, the forgings, shall have workman like surfaces as normally obtained by rolling, forging or drawing.
Provided that the minimum required thickness is maintained, minor surface defects may be admitted and other defects removed by mechanical means so as to achieve a smooth surface. Surface defects may also be repaired, by welding only, with the approval of the Inspecting Authority provided that the parts are stress-relieved after welding where necessary.
Parts of this extracted text look garbled; read the Gazette page before using any value.
Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.
In short
Regulation 58 sets steelmaking, chemistry, heat treatment and surface requirements for forgings of carbon, alloy, stainless steel and nickel alloys.
Key points
- (1) Steel is made by an Open Hearth, Electric or basic Oxygen process, or any process giving equivalent properties.
- (2)(a) Sulphur or phosphorus must not exceed 0.05 per cent.
- (2)(b) Chemistry follows Table 2/35, which covers SA 266, SA 350, SA 105, SA 182, SA 234, SA 336 and nickel alloy N06617 grades. Single values are maximums. The notes add limits, such as caps on combined residual elements for SA 234 WPB and WPC fittings and SA 350 LF1, LF2 and SA 105 forgings, and titanium or columbium minimums linked to carbon for F 321, F 321H and F 347H.
- (3) Heat treatment follows the relevant material specification.
- (4) Unmachined forgings must have workmanlike surfaces as normally obtained by rolling, forging or drawing.
Watch out
- Minor surface defects may be admitted, and other defects removed mechanically to a smooth surface, only if the minimum required thickness is maintained.
- Weld repair of surface defects needs the Inspecting Authority's approval, and parts must be stress-relieved after welding where necessary.
- Table 2/35 is badly misaligned in the extracted text. Check the Gazette page for the exact limits.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
No candidate heading found in the historical print edition.
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.



Indian Boiler Regulations, 2026, reg. 58, Regulation 58, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.544–546. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).