532.Cladded Specimen.─ (1) The corrosion resistant or hard facing overlay weld surface shall be examined by the liquid penetrant method and shall meet the acceptance standards in sub-regulation (2) of regulation164.
(2)The corrosion resistant test coupon shall be sectioned to make four side‐bend (B1, B2, B3, B4) test specimens perpendicular to the direction of the welding as per regulations 160 and 161. Test specimens shall be removed at locations specified in Fig. 13/8.
Plate size 150x150 X T (Base metal thickness) mm
FIG. 13 / 8: ORDER OF REMOVAL OF TEST SPECIMEN FROM CORROSION RESISTANT OVERLAY FOR INITIAL / RE-QUALIFICATION TEST
(3)(a) The hard facing overlay base metal shall be sectioned transversely to the direction of the hard‐facing overlay.
(b)The two faces of the hard‐facing exposed by sectioning shall be polished and etched with a suitable etchant and shall be visually examined with 5X magnification.
(c)Cracks, lack of fusion, or other linear defects in the weld metal or the heat‐affected zone shall be examined (see Fig. 13/9).
Plate size 150x150 X T (Base metal thickness)
FIG. 13/ 9: ORDER OF REMOVAL OF MACRO TEST SPECIMEN FROM HARD FACING OVERLAY FOR INITIAL / RE QUALIFICATION TEST
In short
Regulation 532 sets how cladding (weld overlay) test specimens are examined.
Key points
- (1) Examine the overlay surface by liquid penetrant. It must meet the acceptance standards in sub-regulation (2) of regulation 164.
- (2) Corrosion-resistant overlay: section the coupon into four side-bend specimens (B1 to B4) perpendicular to the welding direction, tested under regulation 160 and regulation 161. Take them from the locations in Fig. 13/8.
- (3) Hard-facing overlay:
- section the base metal across the direction of the overlay;
- polish and etch the two exposed faces, then examine them visually at 5X magnification;
- examine for cracks, lack of fusion and other linear defects in the weld metal or heat-affected zone (Fig. 13/9).
- The figures show a plate size of 150x150 X T, where T is the base metal thickness.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
No candidate heading found in the historical print edition.
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.


Indian Boiler Regulations, 2026, reg. 532, Regulation 532, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.851–852. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).
The citation refers to the government publication. Cite the Gazette, not this website.