Indian Boiler Regulations, 2026 · Chapter 6 · Boiler and Superheater Tubes, Headers and Other Parts
Regulation 244. Regulation 244
Not yet checked against the official Gazette; verify before relying on it.
244.(1)(a)(i) The maximum allowable working pressure of the tubes shall be determined by the following
formula: -
2f (T – C)
P = ---------------- Equation (6/1)
[D – (T - C)]
Where, minimum thickness of tubes, that is, nominal thickness less the permissible negative
T = tolerance in mm,
0.75 mm for working Pressure up to and including 70 kg/cm2 (g)or
C = 0 for working Pressure exceeding 70 kg/cm2 (g).
C = Maximum allowable working Pressure of boiler in kg/cm2 (g),
P = External diameter of tube in mm,
D = maximum permissible stress values as available in the governing codes of the country
f = of the material to which it belongs in kg/cm2. In case of non-availability of the value,
the following procedure for evaluating the permissible stress values shall be adopted.
(ii)The minimum required thickness of tubes shall be determined by the following formula:
t= PxD +C Equation (6/2)
2 x f + P
Where, minimum thickness of tube in mm,
t = 0.75 mm for working pressure up to and including 70 kg/cm2 (g)or
C = 0 for working pressure exceeding 70 kg/cm2 (g).
C = maximum allowable working Pressure of boiler in kg/cm2 (g),
P = External diameter of tube in mm,
D = f = maximum permissible stress values as available in the governing codes of the country of the material to which it belongs in kg/cm2. In case of non-availability of the value, the following procedure for evaluating the permissible stress values shall be adopted.
(A) For temperature at or below 454°C,
Ts Et --- or ----- whichever is lower 2.7 1.5
(B) For temperature above 454°C
Sr Sc whichever is lower
--- or
1.6
Where Ts = minimum tensile strength of the material at room temperature, Et = yield point (0.2 % proof stress) at working metal temperature ‘t’,
Sr = the average stress to produce rupture in 100,000 hours and in no case more than 1.33 times the lowest stress to produce rupture at the working metal temperature,
Sc = the average stress to produce an elongation of 1 percent (creep) in 100,000 hours, at the working metal temperature.
Note: In case Sc values are not available in Material Standard and such materials are known to have been used in boilers in India or abroad, then for such materials the allowable stress may be taken as the lower of
| Et | Sr | |
| ---- 1.5 | or | ----- 1.6 |
Table structure read from the Gazette PDF, page 642. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Et Sr ---- or ----- 1.5 1.6
(b)The working metal temperature shall be taken as following, namely:-
(i)for integral economiser tubes, the maximum water temperature for which the part of the element is designed plus 11°C.
(ii)for furnace and boiler tubes, the saturation temperature corresponding to the working pressure plus 28°C.
(iii)for convection super heater tubes, the maximum steam temperature for which the part of the element is designed plus 39°C.
(iv)for radiant super heater tubes the design maximum steam temperature plus 50°C.
(2)However, in no case, the thickness of tubes as supplied shall be less than those given in the table below (subject to tolerances specified in sub-regulation (5) of regulation 47 and sub-regulation (5) of regulation 49:
TABLE 6/1
| Serial No. | Outside diameter | Seamless Hot finished | Seamless Cold drawn or electric resistance welded |
|---|---|---|---|
| (1) | (2) | (3) | (4) |
| 1. | Upto and including 32 mm | 2.9 mm | 2.03 mm |
| 2. | Over 32mm upto and including 51 mm | 3.25 mm | 2.34 mm |
| 3. | Over 51mm upto and including 76 mm | 3.35 mm | 2.64 mm |
| 4. | Over 76 mm upto and including 89 mm | 3.25 mm | 3.25 mm |
| 5. | Over 89 mm upto and including114 mm | 3.66 mm | 3.66 mm |
Table structure read from the Gazette PDF, page 642. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Serial Outside diameter Seamless Hot finished Seamless Cold drawn or
No. electric resistance welded
(1) (2) (3)
Upto and including 32 mm 2.9 mm (4)
1. 2.03 mm
2. Over 32mm upto and including 3.25 mm 2.34 mm
2.64 mm
51 mm 3.25 mm
3.66 mm
3. Over 51mm upto and 3.35 mm
including 76 mm
4. Over 76 mm upto and 3.25 mm
including 89 mm
5. Over 89 mm upto and 3.66 mm
including114 mmIn the case of coiled tubes for boilers of forced circulation type, the minimum thickness of tubes as supplied may, however, shall be as follows:
Original extracted text of the table above, continued (diagnostic)
Serial No. Table 6/2 Minimum
| Serial No. | Outside diameter of tubes in mm | Minimum thickness |
|---|---|---|
| (1) | (2) | (3) |
| 1. | Upto and including 29 mm. | 1.62 mm. |
| 2. | Over 29 mm. Upto and including 35 mm. | 1.83 mm. |
| 3. | Over 35 mm. upto and including 42 mm | 2.34 m. |
Table structure read from the Gazette PDF, page 643. Verification status as for the text above.
Show original extracted text (diagnostic, not authoritative)
Outside diameter of tubes in mm thickness
(1)
1. (2) (3)
Upto and including 29 mm. 1.62 mm.
2. Over 29 mm. Upto and including 35 mm. 1.83 mm.
2.34 m.
3. Over 35 mm. upto and including 42 mm(3)(a) Tubes that are hot or cold bent for parts of boilers, including economizers, furnace walls, superheaters and reheaters, shall comply with this clause and suitably heat treated as under:
For Carbon steel / Alloy steel (except P-91 and Austenitic Stainless steel) - If percentage thinning is more than 25% - Post Bend Heat Treatment (PBHT) required. - If Outer Diameter (OD) is less than 141.3 mm and R/D ≤ 1.30 – PBHT required. - If Outer Diameter (OD) is more than 141.3 mm and R/D ≤ 2.5 – PBHT required.
For P-91 and Austenitic stainless steel – requirements as specified in the material specifications shall be followed.
Where, R is the mean radius of the bend to the centre line of the tube (in mm) and D is the outside diameter of the tube (in mm).
Butt welds shall not be permitted within bends.
Thinning and departure from circularity limits shall be demonstrated by one of the following methods.
(a)relevant and satisfactory service experience;
(b)a procedure test;.
(c)by measurement of 2% of the bends, including the first bend of each shift.
The method selected shall be at the option of the manufacturer.
(b)Thinning on tube bends shall comply with the following:
(i)At any location around the bend extrados, the reduction in thickness (in per-cent) below the calculated minimum permissible design thickness of the straight tube, except where permitted by (ii), shall not exceed:
_100_
4R + 2
D
Where,
R is the mean radius of the bend to the centre line of the tube (in mm). D is the ordered outside diameter of the tube (in mm).
(ii)Bend thickness below the minimum value required under (i) shall be permitted in cases where the manufacturer can demonstrate by bursting tests carried out on at least three bends that the strength of the bend is not less than that of the straight tube.
(iii)Where the amount of thinning at any location around the bend extrados on cold formed bends exceeds 25% of the actual thickness of the tube on the straight the bends shall be suitably heat treated. The actual thickness of the same plans as the line of the extrados at each end of the bend.
(c)The departure from circularity at the bend apex shall not exceed 10% for bends performed in a single bending operation and 15% for bends which are hot pressed after the primary, bending operation.
The departure from circularity (in percent) shall be calculated from:
Dmax - Dmin x 100
--------------------
D
Where, is the maximum outside diameter measured in the tube bend apex (mm), Dmax=
Dmin= is the minimum outside diameter measured at the same cross section As Dmax (mm)
D is the ordered outside diameter of the tube (in mm).
Parts of this extracted text look garbled; read the Gazette page before using any value.
Tables and formulae are shown in their extracted layout. Alignment, superscripts and subscripts may be lost. The Gazette page image is authoritative.
Tube MAWP and minimum thickness (Equations 6/1 and 6/2, Tables 6/1 and 6/2)
In short
Regulation 244 sets out how to calculate the working pressure and minimum thickness of boiler tubes, the minimum "as supplied" tube thickness, and the rules for bending tubes (heat treatment, thinning and out-of-roundness).
Key points
- (1)(a)(i) Working pressure, Equation (6/1), and (1)(a)(ii) minimum thickness, Equation (6/2). Both use tube thickness, outside diameter D, permissible stress f and an allowance C, which is 0.75 mm for working pressure up to and including 70 kg/cm2 (g) and 0 above that. The symbol list is misaligned in the extracted text, so check the Gazette page for the exact definitions.
- Permissible stress f is taken from the governing code of the material's country. If not available: at or below 454°C use the lower of Ts/2.7 or Et/1.5; above 454°C use the lower of Sr/1.6 or Sc. Sr and Sc are based on 100,000 hours; Sr is capped at 1.33 times the lowest rupture stress. A note covers materials without Sc values (lower of Et/1.5 or Sr/1.6).
- (1)(b) Working metal temperature: integral economiser tubes, design water temperature plus 11°C; furnace and boiler tubes, saturation temperature plus 28°C; convection superheater tubes, design steam temperature plus 39°C; radiant superheater tubes, design steam temperature plus 50°C.
- (2) Minimum as-supplied thickness by outside diameter (Table 6/1), with a separate Table 6/2 for coiled tubes of forced circulation boilers. Both tables are broken in the extracted text; check the Gazette page for the values.
- (3)(a) Bends: for carbon and alloy steel (except P-91 and austenitic stainless), post bend heat treatment (PBHT) is needed if thinning is more than 25%, or if R/D ≤ 1.30 for OD less than 141.3 mm, or R/D ≤ 2.5 for OD more than 141.3 mm. As printed, an OD of exactly 141.3 mm falls in neither case; check with the Inspecting Authority. P-91 and austenitic stainless follow their material specifications.
- (3)(b) Thinning at the extrados is limited by a formula in R and D, unless burst tests on at least three bends show the bend is as strong as the straight tube.
- (3)(c) Out-of-roundness at the bend apex: not more than 10% for single-operation bends and 15% for bends hot pressed after primary bending.
Watch out
- Butt welds are not permitted within bends.
- Thinning and circularity must be demonstrated by service experience, a procedure test, or measuring 2% of bends including the first bend of each shift, at the manufacturer's option.
- Cold formed bends with thinning over 25% of the actual straight-tube thickness must be heat treated.
Written by IBRsource editors · last edited 2026-11-20. Explanations simplify and are not a design method, testing procedure or authorisation. Requirements come from the complete regulations, the Gazette and approved documentation.
Comparison pending: the IBR 1950 text in force on 30 September 2026 is not yet established for this provision, so no change is claimed (how this works).
Orientation hints (unverified)
These candidates come from automated heading matching against DPIIT's scanned historical print edition of IBR 1950. That edition uses imperial units and riveted-construction provisions, so it is not the operative 2026 predecessor text. Regulation numbers alone never prove equivalence.
No candidate heading found in the historical print edition.
Images of the official Gazette pages that contain this regulation. Click to zoom. Compare word by word before relying on the extracted text.




Indian Boiler Regulations, 2026, reg. 244, Regulation 244, Gazette of India, Extraordinary, Part III—Section 4, No. 596, 1 October 2026, printed p.641–644. https://egazette.gov.in/WriteReadData/2026/276813.pdf (text consulted via IBRsource, 2026-11-23).