Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 561
Text in the DPIIT web edition
Archived copy captured 03 Aug 2022 (Wayback Machine); the same page also prints regulations 561A, 561B. The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.
| Reg. 561 a, Reg. 561 b | ||||||||||||||||||
Reg. 561
| ||||||||||||||||||
| ||||||||||||||||||
Earlier text: the 2008 DIPP web edition
(b)Test for Class I boilers
i)Specimens for the following tests shall be selected from the test plate or plates and stamped by the Inspecting Officer for identification (see Figures XII/58 and XII/59): One tensile test specimen for the welded seam.
One all weld metal tensile test specimen.
Two bend test specimens.
Two impact test specimens.
One specimen from each test plate for macro and micro examinations.
The dimensions of the specimens shall be in accordance with the sketches in Figures XII/60, XII/62, XII/63 and XII/64. The remainder of the test plates shall be retained for re-tests if required. Any specimen for re-test shall be cut from the same test plate as the original specimen. Specimens representing welded seams shall, if necessary, be straightened cold before the commencement of machining. Tensile
and bend specimens shall, if practicable, be of the full plate thickness. Surfaces of tensile, bend and Izod specimens corresponding with the outside or inside of the boiler shall be lightly dressed only so that the rolled surface of the parent metal is not wholly removed. Where the rolled surfaces of the abutting plates are not level with one another one plate may be machined at each face of the weld so long as the depth of the metal removed does not exceed 1/32 inch.
ii)Tensile tests:-
(a)(i) Welded joint: –
The dimensions of the reduced tensile section shall be as shown in the Fig 60-1(a).The width of the reduced section shall be at least 25 millimetres.
(ii)If the thickness of the plate does not exceed 30 millimetres, the thickness of the specimen shall be equal to the plate thickness and the plate surface of the specimen shall be machined to take away the surface irregularities of the plate and the weld.
(iii)If the plate thickness exceeds 30 millimetres, the tensile test shall be carried out on several reduced section specimens, each having a thickness of at least 30 millimetres and width at the effective cross-section of at least 25 millimetres. These specimens shall be taken out of the test piece in such a way that the tensile test covers the whole thickness of the weld joints as shown in Fig 60-1(b) . The tensile strength shall not be less than the lower limit specified for the plate.
(b)All weld metal:–
The dimensions of the weld metal tensile test specimen shall be these given in figure 63. The diameter shall be the maximum possible consistent with the cross section of the weld but in no case more than 20 millimetres, the gauge length shall be equal to five times the diameter. The tensile strength shall not be less than the lower limit specified for the plate. The elongation shall not be less than 20 per cent on a gauge length of five times the diameter of the specimen or 5.65 times the square root of the crosssectional area of the specimen, and the reduction in area not less than 35 per cent.
iii)Cold bend tests:- Two bend tests shall be made.
One specimen shall be tested with the outer surface of the weld in tension, and the other with the inner surface in tension. The specimens shall be rectangular in section and shall be cut out transversely to the weld so as to have a width not less than one-and-a half times the thickness of the plates. The sharp corners of the specimens shall be rounded to a radius not exceeding 10% of the thickness of the specimen.
Where the plate thickness does not exceed 1 ¼ inches, the thickness of the specimen shall be equal to the full thickness of the test plate. Where the plate thickness exceeds 1 ¼ inches, the specimen shall in all cases have a thickness of at least 1 ¼ inches. The specimen to be tested with the outer surface of the weld in tension shall be prepared by cutting to waste the metal local to the inner surface of the weld, so that the desired specimen thickness is obtained (see A, Figure XII/64).
The specimen to be tested with the inner surface in tension shall be prepared by cutting to waste the metal local to the outer surface of the weld so that the desired specimen thickness is obtained (see B, Figure XII/64). Where the thickness of the plate permits, both specimens may be cut from the same piece of plate, the specimens being located in the plate one above the other (see C, Figure XII/64). Each specimen shall be mounted with the weld midway between the supports set apart at a distance of not more than 5.2 times the thickness of the specimen and pushed through the supports with a former having a diameter equal to three times the thickness of the specimen.
On completion of the test no crack or defect at the outer surface of the specimen shall be greater than 1/16 inch measured cross the specimen or 1/8 inch measured along the length of the specimen. Premature failure at corners of the specimen shall not be considered cause for rejection.
On completion of the test no crack or defect at the outer surface of the specimen shall be greater than 1/16 inch measured cross the specimen or 1/8 inch measured along the length of the specimen. Premature failure at corners of the specimen shall not be considered cause for rejection.
Next >>>
Amendments found
Machine-assisted list from the amending notifications (DPIIT copies; 1990–1998 from scanned Gazette issues on India Code); may be incomplete.
| Date | Notification | Part | Action | What changed (summary) | Web edition |
|---|---|---|---|---|---|
| 1997-03-19 | G.S.R. 172 OCR of scan | (b)(ii) | Substituted | Replaces clause (ii) on tensile tests: reduced-section welded-joint specimens and all-weld-metal specimens with strength, elongation and area-reduction limits. Uncertain: Regulation number '561' not cross-checked. | listed before the capture |
| 1997-03-19 | G.S.R. 172 OCR of scan | (b)(v) | Substituted | Replaces clause (v) on macro and micro examination of a full-thickness weld specimen. | listed before the capture |
| 1997-03-19 | G.S.R. 172 OCR of scan | figure XII/60(?) | Substituted | Replaces a figure with Specimen Ia/Ib reduced section tensile specimen figure. Uncertain: Replaced figure number garbled ('Xll/h('); new figure caption reads 'Figure XII/61' while text cites 'figure 60-1(a)/(b)'. | listed before the capture |
| 1997-03-19 | G.S.R. 172 OCR of scan | figure XII/63 | Substituted | Replaces Figure XII/63, tensile test all-weld-metal specimen. Uncertain: Printed 'X11/3' in instruction; caption reads XII/63. | listed before the capture |
| 1999-07-21 | G.S.R. 237 | (b)(ii)(b) | Amended | Changes the specimen gauge length to five times the diameter or 5.65 times the square root of the cross-sectional area. | listed before the capture |
| 2005-01-19 | G.S.R. 32 | (b)(viii) | Inserted | Inserts Note (3) requiring non-destructive examination of butt welded joints. | listed before the capture |
| 2006-08-07 | G.S.R. 201 | (a) | Amended | Removes the 16-feet shell length condition for locating the test plate at one end. | listed before the capture |
| 2010-10-07 | G.S.R. 821(E) | Amended | Replaces 'Inspecting officer(s)' with 'Competent Person' wherever it occurs. | listed before the capture | |
| 2010-10-07 | G.S.R. 821(E) | Amended | Replaces 'Inspector' with 'Competent Person' wherever it occurs. | listed before the capture | |
| 2010-10-28 | G.S.R. 195 | (b)(iv) | Amended | Changes the impact test temperature to 20 plus or minus 2 degrees C. | listed before the capture |
| 2015-04-15 | G.S.R. 286(E) | (b)(iv) | Substituted | Replaces clause (iv) on impact tests. | listed before the capture |