Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 561A — Tests on welded seams
Text in the DPIIT web edition
Archived copy captured 03 Aug 2022 (Wayback Machine); the same page also prints regulations 561, 561B. The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.
| Reg. 561 a, Reg. 561 b | ||||||||||||||||||
Reg. 561
| ||||||||||||||||||
| ||||||||||||||||||
Earlier text: the 2008 DIPP web edition
Tests on welded seams
(a)Test Plates
Test plates to represent all welded seams shall be attached at each end of each longitudinal seam in tension. These shall be of a size sufficient for the preparation of the test pieces specified. In the case of shell plates up to an including 16 feet in length the test plate may be located at one end only (see Figure XII/58). Where the shell is formed in two or more rings, the staggered longitudinal seam shall be regarded as a continuous longitudinal seam provided the welding be effected in one reasonably continuous operation and by the same operator or operators. The material for the test plates shall be cut from the respective plate or plates forming the appropriate seam.
In the case of insufficient material being available on the shell plate to permit the cutting of test pieces, these shall be acceptable if they are made from another plate provided it is made from the same cast. The test plates shall be stamped by the Inspecting Authority before being cut.
The weld groove in the test plates shall be similar to that adopted for the corresponding edges of the longitudinal seam, and the respective fusion faces shall be in continuous alignment. The test plates may be reinforced or supported during welding so that any relative displacement due to warping during welding does not exceed 5 degrees. The weld metal in the test plates and the seam shall be deposited continuously at the same operation.
The weld in any test plate shall not be repaired. If any defects are revealed in the weld metal of a test plate the position of this shall be clearly marked on the plate and the test pieces shall be selected from such parts of the test plates as may be decided by the Inspecting Authority.
Test plates warped during welding by not more than 5 degrees may be straightened before heat-treatment. For the heat-treatment of the test plates see Regulation 562.
Where there are circumferential seams only or where the method of welding the circumferential seams differ from that employed for the longitudinal seams, the method of providing the test plates shall be decided by the Inspecting Authority.