Regulation 77 — Tensile Test

Unofficial DPIIT web edition · not verified0 amendments found

Text in the DPIIT web edition

Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.

Unofficial DPIIT web edition · archived 2022 · not checked against the Gazette
Reg. 77
MATERIALS OF CONSTRUCTION

STEEL CASTING


Tensile Test


(a) The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength at room temperature.

(b) A proportional test piece with Lo = 5 do shall be used as test specimen.

(c) The minimum values of stress at proof limit 0.2% at elevated temperature Et of the material may be calculated by multiplying the minimum specified tensile strength at room temperature R20 by the value of ratio Et/R20 given in table under regulation 16.

(d) The breaking elongation in % shall be not less than  93 - Rm
                                                                                                         2.2 

Where, Rm = measured tensile strength at room temperature in kgf/mm2 ;
93 = a quality index
2.2 = a constant which is valid only when Lo = 5 do
Where, Lo = gauge length
             do = original diameter of the round test piece.

(e) If, however, the tensile tests are carried out on specimens conforming to any other standards, the material will be accepted provided the tensile strength and elongation computed on the basis of the dimension of the test pieces under the regulation shall conform to the above requirements.
Earlier text: the 2008 DIPP web edition

MATERIALS OF CONSTRUCTION

STEEL CASTING

Tensile Test

(a)The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength at room temperature.

(b)A proportional test piece with Lo = 5 do shall be used as test specimen.

(c)The minimum values of stress at proof limit 0.2% at elevated temperature Et of the material may be calculated by multiplying the minimum specified tensile strength at room temperature R20 by the value of ratio Et/R20 given in table under regulation 16.

(d)The breaking elongation in % shall be not less than

93-Rm
_____________
2.2

Where, Rm = measured tensile strength at room temperature in kgf/mm² ;

93 = a quality index
2.2 = a constant which is valid only when Lo = 5 do
Where, Lo = gauge length

do = original diameter of the round test piece.

(e)If, however, the tensile tests are carried out on specimens conforming to any other standards, the material will be accepted provided the tensile strength and elongation computed on the basis of the dimension of the test pieces under the regulation shall conform to the above requirements.