Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 16 — Tensile tests
Text in the DPIIT web edition
Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.
| Reg. 16 MATERIALS OF CONSTRUCTION STEEL PLATES, RIVETS, SECTION AND BARS IN CARBON STEEL |
| (a) The tensile strength of different grades of material shall be within the limits specified in regulation 9 (d). (b) – The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength at room temperature. (c) – The breaking elongation in percentage shall be not less than ( N-Rm)/C Where Rm = Tensile strength at room temperature in kgf/mm2 N = a quality index of 100 for plate thickness upto 50 mm or 95 for plate thickness over 50mm. C = 2.2 for only gauge lengths of L=5 do or L=5.65/ ÖAo Where Lo = gauge length Ao = original cross section of the rectangular test piece. do = original diameter of the round test piece. NOTE: C= 1.9 for gauge lengths of 4 ÖAo for test piece of Appendix-B. (d) – The minimum values of the stress at proof limit 0.2% at elevated temperature (Et) may be calculated by multiplying the minimum specified tensile strength at room temperature (R20) by the value of the ratio (Et/R20) given in the table below: TABLE
*For temperatures lower than 300°C any test required for acceptance purposes (in the absence of records of previous tests at these temperatures) shall be made at 300°C, in which case the proof stress shall be not less than value obtained by calculation from the specified minimum tensile strength at room temperature and the above proof-ratio of 0.36 for 300°C. |
Earlier text: the 2008 DIPP web edition
MATERIALS OF CONSTRUCTION
STEEL PLATES, RIVETS, SECTION AND BARS IN CARBON STEEL
Tensile tests
(a)The tensile strength of different grades of material shall be within the limits specified in regulation 9 (d).
(b)– The upper yield point at room temperature shall be not less than 50% of the specified minimum tensile strength at room temperature.
(c)– The breaking elongation in percentage shall be not less than ( N-Rm)/C
Where Rm = Tensile strength at room temperature in kgf/mm²
N = a quality index of 100 for plate thickness upto 50 mm or 95 for plate thickness over 50mm.
C = 2.2 for only gauge lengths of L=5 do or L=5.65/ √Aο
Where Lο = gauge length
Aο = original cross section of the rectangular test piece.
dο = original diameter of the round test piece.
NOTE: C= 1.9 for gauge lengths of 4 √Aο for test piece of Appendix-B.
(d)– The minimum values of the stress at proof limit 0.2% at elevated temperature (Et) may be calculated by multiplying the minimum specified tensile strength at room temperature (R20) by the value of the ratio (Et/R20)
Minimum values for the ratio of the stress at proof limit 0.2% at elevated temperature (Et) to the minimum specified tensile strength at room temperature (R20) of carbon steel boiler plates.
Temperature 250°C *275°C 300°C 325°C 350°C 375°C Et/R20 0.40 0.38 0.36 0.34 0.33 0.32 Temperature 400°C 425°C Et/R20 0.31 0.30
*For temperatures lower than 300°C any test required for acceptance purposes (in the absence of records of previous tests at these temperatures) shall be made at 300°C, in which case the proof stress shall be not less than value obtained by calculation from the specified minimum tensile strength at room temperature and the above proof-ratio of 0.36 for 300°C.
Amendments found
Machine-assisted list from the amending notifications (DPIIT copies; 1990–1998 from scanned Gazette issues on India Code); may be incomplete.
| Date | Notification | Part | Action | What changed (summary) | Web edition |
|---|---|---|---|---|---|
| 2015-04-15 | G.S.R. 286(E) | (d) | Amended | Bases maximum permissible stress on the governing code of the material's country. | listed before the capture |