BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)

Regulation 338 — BOILER AND SUPER HEATER TUBES, HEADERS AND OTHER PRESSURE PARTS TUBES

Unofficial DPIIT web edition · not verified5 amendments found

Text in the DPIIT web edition

Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.

Unofficial DPIIT web edition · archived 2022 · not checked against the Gazette
Reg. 338

BOILER AND SUPER HEATER TUBES, HEADERS AND OTHER PRESSURE PARTS TUBES

a) The working pressure of the tubes shall be determined by the following formula:-

W. P. = 2 f (T - C) Eqn.(87)

(D - T + C)

where,

T = minimum thickness of tubes, that is, nominal thickness less the permissible negative tolerance in mm. (inch)
C = 0.75 mm for working pressure up to and including 70 kg/cm².

or

C = 0 for working pressure exceeding 70 kg/cm² (1000 lbs/sq. in.)
W. P.= Working pressure of boiler in kg/cm² (lbs/sq. inch)
D = External diameter of tube in mm (inch)
F = permissible stress for the material at the working metal temperature in kg/cm² (lbs/sq. Inch) to be determined on the basis given below:-

The working metal temperature shall be taken as :-

(a) For integral economiser tubes, the maximum water temperature for which the part of the element is designed plus 11°C (20°F).

(b) For furnace and boiler tubes, the saturation temperature corresponding to the working pressure plus 28°C (50o F)

(c) For convection superheater tubes, the maximum steam temperature for which the part of the element is designed plus 39oC (70oF).

(d) For radiant superheater tubes the designed maximum steam temperature plus 50 °C (90oF)

Permissible working stress for tubes:- For temperatures at or below 454 °C,

T. S. or Et whichever is lower.
2.7 1.5

For temperature above 454 °C,

Sr or Sc whichever is lower.
1.5

where,

T.S. = Minimum tensile strength of the material at room temperature.
Et = Yield point (0.2% proof stress) at working metal temperature 't'.
Sr = the average stress to produce rupture in 100,000 hours and in no case more than 1.33 times the lowest stress to produce rupture at the working metal temperature.
Sc = the average stress to produce an elongation of 1% (creep) in 100,000 hours, at the working metal temp.

Note:- In case Sc values are not available in Material Standard and such materials are known to have been used in boilers in India or abroad, then for such material the allowable stress may be taken as the lower of

Et or Sr
1.5 1.5
b)

In no case, however, shall the thickness of tubes as supplied be less than those given in the table below (subject to tolerances specified in Regulations 36(d), 43(d), 48(c), 53(c), 56A (IV) and 58(d).

TABLE

Outside diameter Seamless Hot finished Seamless Cold drawn or electric resistance welded
Upto to and including 32 mm. (1 ¼" )..... 2.9 mm.
(0.116in.)
2.03mm.
(0.08in.)
Upto to and including 51 mm.(2")... 3.25mm.
(0.128in)
2.34mm
(0.092in.)
Over 51 mm (2in.) Upto and including 76mm.(3in.) 3.35mm.
(0.128in.)
2.64mm.
(0.104in.)
Over 76mm.(3in.) Upto and including 89mm. (3-1/2in.) 3.25mm.
(0.128in.)
3.25mm.
(0.128in.)
Over 89mm.(3-1/2in.) Upto and including114 mm.- (4 ½ in.) 3.66mm.
(0.144in.)
3.66mm.
(0.144in.)

In the case of coiled tubes for boilers of the forced flow or forced circulation type, the minimum thickness of tubes as supplied may, however, be as follows:-

Outside diameter of tubes in inches Minimum thickness
Up to and including 29mm.(13") 1.62mm. (O.064")
Over 29mm. up to and including 35mm. (1 3/8”) 1.83mm. (0.072')
Over 35 mm. (1 3/8") up to and including 42mm.(1 5/8") 2.34mm. (0.092)
c)

(i) General: Tubes that are hot or cold bent for parts of boilers, including economizers, furnace walls, superheaters and reheaters, shall comply with this clause and suitably heat treated. 

Butt welds shall not be permitted within bends.

Thinning and departure from circularity limits shall be demonstrated by one of the following methods. 

(a) relevant and satisfactory service experience;

(b) a procedure test;.

(c) By measurement of 2% of the bends, including the first bend of each shift.

The method selected shall be at the option of the manufacturer.

(ii) Thinning on tube bends.  Thinning on tube bends shall comply with the following.

(a) At any location around the bend extrados, the reduction in thickness (in percent) below the calculated minimum permissible design thickness of the straight tube, except where permitted by (b), shall not exceed:

          __100___

             4R + 2                                    

              D

where

R is the mean radius of the bend to the centre line of the tube (in mm).

D is the ordered outside diameter of the tube (in mm).

               (b) Bend thickness below the minimum value required under (a) shall be permitted in cases where the manufacturer can demonstrate by bursting tests carried out on at least three bends that the strength of the bend is not less than that of the straight tube.

               (c) Where the amount of thinning at any location around the bend extrados on cold formed bends exceeds 25% of the actual thickness of the tube on the straight the bends shall be suitably heat treated.  The actual thickness of the same plans as the line of the extrados at each and of the bend.

(iii)  Departure from circularity in tube bends.  The departure from circularity at the bend apex shall not exceed 10% for bends performed in a single bending operation and 15% for bends which are hot pressed after the primary, bending operation.

The departure from circularity (in percent) shall be calculated from:

 Dmax - Dmin  ´ 100

                   D

where

Dmax is the maximum outside diameter measured in the tube bend apex (mm),

Dmin is the minimum outside diameter measured at the same cross section as Dmax(mm)

D     is the ordered outside diameter of the tube (in mm).

 

d) For radiant superheater tubes, the maximum steam temperature for which the part of the element is designed plus 50°C (90°F).
Earlier text: the 2008 DIPP web edition

BOILER AND SUPER HEATER TUBES, HEADERS AND OTHER PRESSURE PARTS TUBES

a)The working pressure of the tubes shall be determined by the following formula:-

                                           2 f (T - C)            Eqn.
W. P. =
                                           (D - T + C)            (87)
where,

T = minimum thickness of tubes, that is, nominal thickness less the permissible negative tolerance in mm. (inch)

C = 0.75 mm for working pressure up to and including 70 kg/cm².

or

C = 0 for working pressure exceeding 70 kg/cm² (1000 lbs/sq. in.)

W. P.= Working pressure of boiler in kg/cm² (lbs/sq. inch)

D = External diameter of tube in mm (inch)

F = permissible stress for the material at the working metal temperature in kg/cm² (lbs/sq. Inch) to be determined on the basis given below:-

The working metal temperature shall be taken as :-

(a)For integral economiser tubes, the maximum water temperature for which the part of the element is designed plus 11°C (20°F).

(b)For furnace and boiler tubes, the saturation temperature corresponding to the working pressure plus 28°C (50o F)

(c)For convection superheater tubes, the maximum steam temperature for which the part of the element is designed plus 39oC (70oF).

(d)For radiant superheater tubes the designed maximum steam temperature plus 50 ° C (90oF)

Permissible working stress for tubes:- For temperatures at or below 454 °C,

T. S.                          Et
                or                         whichever is lower.
 2.7                           1.5

For temperature above 454 °C,

Sr
               or           Sc          whichever is lower.
1.5

where,

T.S. = Minimum tensile strength of the material at room temperature.

Et = Yield point (0.2% proof stress) at working metal temperature 't'.

Sr = the average stress to produce rupture in 100,000 hours and in no case more than 1.33 times the lowest stress to produce rupture at the working metal temperature.

Sc = the average stress to produce an elongation of 1% (creep) in 100,000 hours, at the working metal temp.

Note:- In case Sc values are not available in Material Standard and such materials are known to have been used in boilers in India or abroad, then for such material the

allowable stress may be taken as the lower of

 Et                                          Sr
                       or
1.5                                          1.5

b)In no case, however, shall the thickness of tubes as supplied be less than those given in the table below (subject to tolerances specified in Regulations 36(d), 43(d), 48(c), 53

(c), 56A (IV) and 58(d).

                                 TABLE

                                                       Seamless Cold
                                       Seamless Hot
Outside diameter                                      drawn or electric
                                         finished
                                                     resistance welded
                                          2.9 mm.         2.03mm.
Upto to and including 32 mm. (1 ¼" ).....
                                         (0.116in.)       (0.08in.)
                                         3.25mm.          2.34mm
Upto to and including 51 mm.(2")...
                                         (0.128in)        (0.092in.)
Over 51 mm (2in.) Upto and including     3.35mm.          2.64mm.
76mm.(3in.)                              (0.128in.)       (0.104in.)
Over 76mm.(3in.) Upto and including      3.25mm.          3.25mm.
89mm. (3-1/2in.)                         (0.128in.)       (0.128in.)
Over 89mm.(3-1/2in.) Upto and            3.66mm.          3.66mm.
including114 mm.- (4 ½ in.)              (0.144in.)       (0.144in.)

In the case of coiled tubes for boilers of the forced flow or forced circulation type, the minimum thickness of tubes as supplied may, however, be as follows:-

        Outside diameter of tubes in inches        Minimum thickness
Up to and including 29mm.(13")                   1.62mm. (O.064")
Over 29mm. up to and including 35mm. (1 3/8”)    1.83mm. (0.072')

Over 35 mm. (1 3/8") up to and including 42mm.(1 5/8") 2.34mm. (0.092)

c)Where tubes are bent, care shall be taken to ensure that the total strain at the bend is not more than that at the straight part of the tube.

The deviation from circularity in percentage at any cross section of a bend shall be calculated by the following formula:-

                           Dmax - Dmin.
C =                                               x      100
                                D

                                      20 D
The deviation shall not exceed
                                      R

where,

C = The percentage deviation of circularity.

Dmax = maximum external diameter of the tube as gauged at the bend.

Dmin. = minimum external diameter of the tube as gauged at the bend.

D = nominal external diameter of the tube.

R = Radius of the bend on the central line of the bend.

d)For radiant superheater tubes, the maximum steam temperature for which the part of the element is designed plus 50°C (90°F).

Amendments found

Machine-assisted list from the amending notifications (DPIIT copies; 1990–1998 from scanned Gazette issues on India Code); may be incomplete.

DateNotificationPartActionWhat changed (summary)Web edition
1995-02-14G.S.R. 83 OCR of scan(a)InsertedInserts the same Note on allowable stress after the explanation of 'Se' ending "working metal temp.".listed before the capture
2001-12-10G.S.R. 672(c)SubstitutedReplaces clause (c) on hot or cold bent tubes, including ovality limits.listed before the capture
2010-10-28G.S.R. 195(b)AmendedCorrects a table entry from 3.35 mm to 3.25 mm.listed before the capture
2015-04-15G.S.R. 286(E)(a)SubstitutedReplaces sub-regulation (a) on working pressure of tubes.listed before the capture
2015-04-15G.S.R. 286(E)(c)(i)SubstitutedReplaces clause (i) on hot or cold bent tubes.listed before the capture