Indian Boiler Regulations, 2026
Appendix E — PROOF TEST FOR CREEP QUALITY OF CARBON STEEL BOILER QUALITY PLATE – SPECIFICATION
Not yet checked against the official Gazette; verify before relying on it.
Open the official Gazette at this appendix
APPENDIX-E
PROOF TEST FOR CREEP QUALITY OF CARBON STEEL BOILER QUALITY PLATE– SPECIFICATION
1. NATURE OF TEST.─ The test shall consist of a tensile creep test carried out over a period of at least 48 hours at a temperature of 450°C and with stress of 11.25 kg/mm2. Under these conditions the slope of the chord to the creep curve between the 24th and 48th hour shall not exceed 50 x 10 = 4° strain per hour.
2. CONDITION OF MATERIAL. ─ The test shall be made on the material in the normalized condition. The normalizing temperature shall be between 875°C – 925°C, and the plate sample shall be maintained at the normalizing temperature for one hour per inch of thickness and cooled freely in still air.
3. TEMPERATURE OF TEST. ─
(1)Temperature Measurement. ─ (a) The temperature of the specimen shall be measured by thermocouples suitable for the temperature specified. Two thermocouples situated one at each end of the gauge length shall be used in the case of test pieces having gauge lengths upto 51 mm, and for longer gauge lengths and additional thermocouple situated at the middle of the gauge length shall be used.
(b)Thermocouples shall make good thermal contact with the test piece and the protected from the direct heat of the furnace of being covered with asbestos tape or equivalent insulation.
(c)The cold junction shall be maintained at a known temperature which shall be registered by a mercury thermometer. Alternatively, a suitable means shall be provided for correcting automatically errors in reading due to changes in temperature of the cold junction.
(2)Temperature Control. ─The two (or three) thermocouples specified in clause (a) shall agree with one another within 3°C and the average of these readings shall be taken as the test temperature which shall not vary from 450°C by more than ± 2°C throughout the test.
Either a continuous record of sufficient readings of the temperature shall be made to indicate that the temperature conditions have been satisfactory.
(3)Heating period before loading. ─ The specimen shall be maintained at the specified temperature for at least an hour prior to the application of the load.
4. STRESS. ─The load required to produce the specified stress shall be gradually applied without shock during a period not exceeding five minutes and the stress shall be accurate to ± 2 ½ percent.
5. SENSITIVITY OF STRAIN-MEASUREING EQUIPMENT. ─The sensitivity of the extensometer must be such that strains can be measured to the nearest 0.00002.
6. READINGS. ─ A sufficient number of strain readings shall be taken clearly to define the creep curve upto 48 hours, and the chord slope shall be measured from a chord drawn between points on the curve at the 24th and 48th hours.
7. REPEAT TEST. ─ If the materials fail to pass the test, but the chord slope does not exceed 60 x 10 = 6° strain per hour, a retest may be made at the request of the manufacturer and shall be accepted if satisfactory, or at the Competent Person discretion a pass test at a stress 5 percent less than that specified may be accepted.
Gazette pages