Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 59 — Flattening test
Text in the DPIIT web edition
Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.
| Reg. 59 MATERIALS OF CONSTRUCTION |
| (a) Flattening test.- (i) A section of the tube not less than 40 mm length shall be flattened cold between parallel plates. No cracks or breaks in the metal shall occur until the distance between the plates is less than the given by the following formula. Evidence of lamination or burnt material or incomplete penetration of the weld shall not develop during the testing. ( 1 + e ) t
H = ----------------
e + ( t /D ) Where t = Specified thickness of tube (in mm) D = Specified outside diameter of tube (in mm) e = Flattening test constant as given below : 0.10 for tube grade WC 1 0.07 for tube grades WC2 & WC3. (ii) The weld shall be placed 90 degree from the line of direction of the applied force. (iii) Superficial rupture as a result of minor surface imperfections shall not be cause for rejection. (iv) Flattening test carried out in accordance with any other standard code may be accepted in which case the code adopted shall be specified. (b) Flaring Test.- A section of tube of length equal to 1.5 times the outside diameter, but not less than 50 mm, shall stand being flared with a tool having 60 or 45 degree included angle until the tube at the mouth of the flare has expanded to the percentage given below without cracking _________________________________________________________________________ Tube % expansion in outside diameter D for a d/D of_______ Grade 0.6 and Over 0.6 to Over 0.8 under 0.8 including_____________________ WC 1 12 15 19 WC2 12 15 19 WC3 10 12 17 _________________________________________________________________ d = inside diameter of tube.
|
Earlier text: the 2008 DIPP web edition
MATERIALS OF CONSTRUCTION
ELECTRICAL -RESISTR|ANCE -WELED STEEL BIOLER AND SUPER-HEATER TUBES FOR DESIGN METAL TEMPERATURES NOT EXCEEDING 454⁰ C (850⁰ F)
Flattening test
(a)Flattening test.- (i) A section of the tube not less than 40 mm length shall be flattened cold between parallel plates. No cracks or breaks in the metal shall occur until the distance between the plates is less than the given by the following formula. Evidence of lamination or burnt material or incomplete penetration of the weld shall not develop during the testing.
( 1 + e ) t
H = ----------------
e + ( t /D )
Where t = Specified thickness of tube (in mm)
D = Specified outside diameter of tube (in mm)
e = Flattening test constant as given below :
0.10 for tube grade WC 1
0.07 for tube grades WC2 & WC3.
(ii)The weld shall be placed 90 degree from the line of direction of the applied force.
(iii)Superficial rupture as a result of minor surface imperfections shall not be cause for rejection.
(iv)Flattening test carried out in accordance with any other standard code may be accepted in which case the code adopted shall be specified.
(b)Flaring Test.- A section of tube of length equal to 1.5 times the outside diameter, but not less than 50 mm, shall stand being flared with a tool having 60 or 45 degree included angle until the tube at the mouth of the flare has expanded to the percentage given below without cracking
Tube Grade % expansion in outside diameter D for a d/D of
0.6 and Over 0.6 to Over 0.8
under 0.8 including
WC1 12 15 19
WC1 12 15 19
WC3 10 12 17
d = inside diameter of tube.
Amendments found
Machine-assisted list from the amending notifications (DPIIT copies; 1990–1998 from scanned Gazette issues on India Code); may be incomplete.
| Date | Notification | Part | Action | What changed (summary) | Web edition |
|---|---|---|---|---|---|
| 1999-10-14 | G.S.R. 345 | Substituted | Replaced as part of the block substitution of regulations 57 to 63A (electrically welded tubes). | listed before the capture |