Regulation 53B — Heat treatment

Unofficial DPIIT web edition · not verified0 amendments found

Text in the DPIIT web edition

Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.

Unofficial DPIIT web edition · archived 2022 · not checked against the Gazette
Reg. 53 b
MATERIALS OF CONSTRUCTION

SEAMLESS FERRITIC PIPES FOR HIGH TEMPERATURE SERVICE

Heat treatment

(i) All pipes of grades in table-1 except P91 and X20CrMoV121 shall be reheated and furnished in full annealed, isothermal annealed or normalised and tempered condition.  If furnished in the normalised and tempered condition, the minimum tempering temperature for grade P1, P2, P11 and P12 shall be 650 degree C and the minimum tempering temperature for grades P5, P9 and P22 shall be 675 degree C.

(ii)  Pipes of grades P1, P2 and P12 either hot finished or cold drawn may be given a final heat treatment at 650 degree C to 705 degree C, instead of heat treatment specified in sub-clause (i) above at the option of the manufacturer.

(iii)  Grades P91 shall be normalised at 1040 degree C minimum and tempered at 730 degree minimum as a final heat treatment.

(iv)  Grades X20CrMoV121 shall be normalised at 1020 - 1070 degree C and tempered at 730-780 degree C for a period of one hour minimum.

Earlier text: the 2008 DIPP web edition

MATERIALS OF CONSTRUCTION

SEAMLESS CHROMIUM-MOLYBDENUM STEEL BOILER AND SUPER HEATER TUBES FOR DESIGN METAL TEMPERATURES NOT EXCEEDING 538 DEGREE C (1,000 DEGREE F).

Heat treatment

The tubes shall be fully annealed or normalised and tempered, at a temperature approved by the Inspecting Authority.