BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)

Regulation 506 — Process of manufacture

Unofficial DPIIT web edition · not verified0 amendments found

Text in the DPIIT web edition

Archived copy captured 03 Aug 2022 (Wayback Machine); the same page also prints regulation 505. The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.

Unofficial DPIIT web edition · archived 2022 · not checked against the Gazette

Reg. 505, Reg. 506
STANDARD CONDITIONS FOR THE DESIGN AND CONSTRUCTION OF ECONOMISER, FEED PIPES, FEED HEATERS AND OTHER SIMILAR VESSELS

ECONOMISERS

Workmanship and manufacture

All material used in the construction of pressure parts shall be tested and shall conform with the following requirements:-

(a) The workmanship throughout shall be of the highest standard. All castings shall be well finished, free from defects porous placed and below holes, and true to dimensions without warping. Where chaplets are used, there must be satisfactory fusion with the metal. Chaplets must be properly tinned with metal free from lead.

(b) The screw threads of all bolts must be of Whitworth forms.

(c) All component parts shall where necessary, be manufactured to limit gauges to secure interchangeability throughout.



Reg. 506
STANDARD CONDITIONS FOR THE DESIGN AND CONSTRUCTION OF ECONOMISER, FEED PIPES, FEED HEATERS AND OTHER SIMILAR VESSELS

CAST IRON, TUBES AND HEADERS

Process of manufacture

(a) The castings shall be cast from metal melted or refined in any suitable metallurgical plant other than an iron ore smelting furnace.

The minimum test results required on test bars 1.2 in. in diameter shall be in accordance with the table

NOTE.-Grade 16.5, 14 and 12 iron correspond to 26, 22 and 18.73 kg/cm² (16, 14 and 12 tons) minimum tensile strength respectively.

(b) On analysis, the sulphur and phosphorous content shall not exceed the following percentages:-

Components 

Sulphur percent
max.

Phosphorus percent max.

Tubes 
Headers
0.15
0.15
1.00
1.00

(c) Minimum Manganese content shall be related to sulphur content by the following formula:-

(% sulphur x 1.7) + 0.3=% Manganese.

Which must be shown to be satisfied by routine quality control laboratory analysis. In any event the Manganese shall not be less than 0.5% and shall be within the range 0.50-0.90%.

Phosphorous content shall be kept as low as economically possible but in no circumstances shall it exceed 1.0%.

Earlier text: the 2008 DIPP web edition

STANDARD CONDITIONS FOR THE DESIGN AND CONSTRUCTION OF ECONOMISER, FEED PIPES, FEED HEATERS AND OTHER SIMILAR VESSELS

CAST IRON, TUBES AND HEADERS

Process of manufacture

(a)The castings shall be cast from metal melted or refined in any suitable metallurgical plant other than an iron ore smelting furnace.

The minimum test results required on test bars 1.2 in. in diameter shall be in accordance with the table

NOTE.-Grade 16.5, 14 and 12 iron correspond to 26, 22 and 18.73 kg/cm² (16, 14 and 12 tons) minimum tensile strength respectively.

(b)On analysis, the sulphur and phosphorous content shall not exceed the following percentages:-

                      Sulphur percent      Phosphorus percent
Components
                           max.                   max.
   Tubes                   0.15                   1.00
  Headers                  0.15                   1.00

(c)Minimum Manganese content shall be related to sulphur content by the following formula:-

(% sulphur x 1.7) + 0.3=% Manganese.

Which must be shown to be satisfied by routine quality control laboratory analysis. In any event the Manganese shall not be less than 0.5% and shall be within the range 0.500.90%.

Phosphorous content shall be kept as low as economically possible but in no circumstances shall it exceed 1.0%.