BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)

Regulation 34 — Stay and Rivet bars

Unofficial DPIIT web edition · not verified0 amendments found

Text in the DPIIT web edition

Archived copy captured 03 Aug 2022 (Wayback Machine). The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.

Unofficial DPIIT web edition · archived 2022 · not checked against the Gazette
Reg. 34
MATERIALS OF CONSTRUCTION

COPPER PLATES, STAY AND RIVET BARS

Stay and Rivet bars

(a) Process.- To comply with  Regulation 33 (a).

(b) Chemical Composition.- To comply with  Regulation 33 (b).

(c) Freedom from Defects.- To comply with  Regulation 33 (c).

(d) Rolling Margin.- The bars in any part shall not be more than 1% over or more than ½% under the specified diameter.

(e) Tensile Tests.- The materials shall have the tensile properties shown in the following table:-

Tensile properties

Unturned rods (rods upto 1¼ inches dia.)
Turned rods (rod above 1¼ inches dia.)
Minimum tensile strength lb. per sq. inch. 32,400 32,400
Elongation, minimum per cent in 2 inches gauge length.
40
45

f) Bend Tests.- To comply with  Regulation 33(f).

(g) Dump Tests.- a piece of rod 1 inch long shall be placed on end and hammered or crushed down cold to a thickness of 3/8 inch without showing either crack or flaw on the circumference of the resulting disc.

(h) Number of Tests.- One bar, from which the required test specimens shall be taken, shall be selected at random from each batch of 50 (or part thereof) bars of each size from each melt. From each bar selected, one tensile test, one cold bend test, one hot bend test and one dump test shall be made.

Earlier text: the 2008 DIPP web edition

MATERIALS OF CONSTRUCTION

COPPER PLATES, STAY AND RIVET BARS

Stay and Rivet bars

(a)Process.- To comply with Regulation 33 (a).

(b)Chemical Composition.- To comply with Regulation 33 (b).

(c)Freedom from Defects.- To comply with Regulation 33 (c).

(d)Rolling Margin.- The bars in any part shall not be more than 1% over or more than ½% under the specified diameter.

(e)Tensile Tests.- The materials shall have the tensile properties shown in the following table:-

Tensile properties

                                Unturned rods (rods    Turned rods (rod above
                                upto 1¼ inches dia.)   1¼ inches dia.)

Minimum tensile strength lb. per
                                32,400                 32,400
sq. inch.

Elongation, minimum per cent in
                                40                     45
2 inches gauge length.

f)Bend Tests.- To comply with Regulation 33(f).

(g)Dump Tests.- a piece of rod 1 inch long shall be placed on end and hammered or crushed down cold to a thickness of 3/8 inch without showing either crack or flaw on the circumference of the resulting disc.

(h)Number of Tests.- One bar, from which the required test specimens shall be taken, shall be selected at random from each batch of 50 (or part thereof) bars of each size from each melt. From each bar selected, one tensile test, one cold bend test, one hot bend test and one dump test shall be made.