Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 307A — Materials
Text in the 2008 DIPP web edition
saved copy p.301, as amended to about 2005 (later amendments below are not merged; units as printed).
SPRINGS AND TORSION BARS
Materials
Springs
The springs shall be manufactured from steel made by the Acid Open Hearth or Electric Process and the Chemical composition shall be within the following limits:
Carbon Steel
Element Per cent
Min. Max
Carbon 0.90 1.20
Silicon 0.30
Manganese 0.45 0.80
Sulphur 0.050
Phosphorus 0.050
Silicon Manganese Steel
Carbon 0.50 0.65
Silicon 1.50 2.00
Manganese 0.70 1.00
Sulphur 0.050
Phosphorus 0.050
Alloy Steel
Grade I Grade II Grade III Grade IV
Carbon % 0.55 to o.65 0.46 to 0.54 0.55 to 0.65 0.55 to 0.65
Manganese % 0.70 to 1.00 0.70 to 0.90 0.70 to 1.00 0.70 to 1.00
Silicon % 0.10 to 0.35 0.10 to 0.35 0.10 to 0.35 1.70 to 2.10
Chromium % 0.60 to 0.90 0.80 to 1.10 0.40 to 0.60 0.20 to 0.40
Molybdenum % - - 0.15 to 0.25 0.20 to 0.30
Vanadium % - 0.15 min - -
Nickel % - - 0.40 to 0.70 -
Phosphorus % - - - -
Sulphur - - - -
The Manufacturers shall supply an analysis of each cast when required by the Inspecting Authority to do so. Should independent analysis be required, these shall be made at the rate of one per cast.
All springs shall be formed hot and suitably hardened and tempered.
All the springs above 16 mm bar diameter shall be formed hot and the springs below 16 mm bar diameter shall be formed hot or cold. The springs shall be suitably hardened and tempered.