Indian Boiler Regulations, 1950 (superseded 1 Oct 2026)
Regulation 234 — MATERIALS OF CONSTRUCTION
Text in the DPIIT web edition
Archived copy captured 03 Aug 2022 (Wayback Machine); the same page also prints regulation 233. The text matches the 2019 capture; amendments from 2020 onwards are probably not included. Units as printed.
|
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
|
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
| |||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||||
Earlier text: the 2008 DIPP web edition
MATERIALS OF CONSTRUCTION
Materials for Fusion Welded Boiler Drums
a)The requirements of Chapter II, so far as they relate to plates, shall apply, excepting that the chemical composition tensile strength and elongation of the material used shall conform to the following, as may be applicable to the quality of steels concerned:
Carbon steels Chemical Composition (ladle analysis) *Carbon 0.25% maximum Silicon 0.35% maximum Manganese 0.40 to 0.90% Phosphorus 0.05% maximum Sulphur 0.05% maximum
*A carbon content not exceeding 0.35% may be permitted, subject to the approval of the Inspecting Authority.
Manganese Steels
Carbon 0.23% maximum Silicon 0.15 to 0.60% Manganese 0.90 to 1.40% Phosphorus 0.05% maximum Sulphur 0.05% maximum
Molybdenum Steels
Carbon 0.21% maximum Silicon 0.15 to 0.35% Manganese 0.50 to 0.90% Phosphorus 0.05% maximum Sulphur 0.05% maximum Molybdenum 0.25 to 0.60%
Chromium-Molybdenum Steels
Carbon 0.21% maximum Silicon 0.15 to 0.35% Manganese 0.40 to 0.80% Phosphorus 0.04% maximum Sulphur 0.04% maximum Chromium 0.7 to 1.15% Molybdenum 0.40 to 0.65%
Mechanical Properties at 20°C (68°F)
Kind of Steel Tensile strength minimum *elongation on
Lo=5do or
Lo=5.65(Ao)¹ᐟ²
kg/mm² tons/sq.in. % minimum
Carbon Steels:
(1) 35 22 22
(2) 38.5 24.5 21
(3) 41 26 20
(4) 44 28 19
(5) 47 30 18
Manganese Steels:
(1) 47 30 18
(2) 52 33 16
Molybdenum Steels 44 28 19
Chromium-Molybdenum Steels 42 27 20
*Note:-
Lo = original gauge length;
Do = original diameter, and
Ao = original area of cross section.
NOTE:- A range of not more than 20 per cent of the minimum tensile strength shall be permitted in each class of material.
b)Plates over 2” in thickness before being fabricated, shall be uniformly heat treated to produce grain refinement. Heat treatment involving quenching in a liquid medium is not permitted.