BETAIndependent engineering reference. Source-text verification is ongoing.Verification ongoing.Verification status →
IBRsourceIndian Boiler Regulations, made clear

Historical amendment to IBR 1950 — superseded by IBR 2026 on 1 Oct 2026, subject to the savings provisions

Indian Boiler (Amendment) Regulations, 2001

Official text — not yet verifiedG.S.R 219Notification dated 10th April, 2001
What it amends (editorial summary, pending verification)

Substitutes IBR 1950 regulations 36 to 56 with new provisions for seamless tubes and pipes: cold drawn carbon steel boiler tubes, carbon steel pipes, and ferritic and austenitic alloy steel tubes and pipes, with tables.

Official Gazette PDF (DPIIT). Regulation numbers below refer to the IBR 1950, not the IBR 2026.

IBR 1950 regulation numbers appearing in the notification (includes incidental references; verification pending): —

Not yet checked against the official notification; verify before relying on it.

Official text · Gazette notification · English portion · verification status above

New Delhi, the 10th April, 2001.

Notification

G.S.R 219.- Whereas certain draft regulations, further to amend the Indian Boiler Regulations, 1950, were published, as required by sub-section (1) of section 31 of the Indian Boilers Act, 1923 (5 of 1923), at pages 3755 to 3789 in Part II, Section 3, Sub-section (i) of the Gazette of India, dated the 23rd December, 2000 vide notification of the Government of India in the Ministry of Commerce and Industry (Department of Industrial Policy and Promotion) (Central Boilers Board) number G.S.R. 512, dated the 12th December, 2000 for inviting objections and suggestions from persons likely to be affected thereby till the expiry of forty-five days from the date on which copies of the Gazette containing the said notification were made available to the public;

And whereas the copies of the said Gazette were made available to the (general) public on the 27th day of December, 2000;

And whereas no objections or suggestions were received within the specified period;

Now, therefore, in exercise of the powers conferred by section 28 of the Indian Boilers Act, 1923, the Central Boilers Board hereby makes the following regulations further to amend the Indian Boiler Regulations, 1950, namely:-

1. (1) These regulations may be called the Indian Boiler (Amendment) Regulations, 2001.

(2)They shall come into force on the date of their publication in the Official Gazette.

2. In the Indian Boiler Regulations, 1950, for regulations 36 to 56, the following regulations shall be substituted, namely : -

"COLD DRAWN SEAMLESS CARBON STEEL BOILER, SUPERHEATER
AND HEAT EXCHANGER TUBES FOR DESIGN METAL TEMPERATURES
NOT EXCEEDING 454 DEGREE C (850 DEGREE F)

36.(a) General.- (i) These regulations cover both hot finished and cold drawn seamless boiler, superheater and heat exchanger tubes, which shall conform in all respects with the requirements herein specified.

(ii)The seamless tubes conforming to other national or international standards which are known to be commonly used as being suitable for use as boiler, superheater and heat exchanger tubes can also be used with the designations of the national or international standards, provided such materials are not specifically prohibited by the regulations.

2

(iii)While making tubes to other national/international standards the allowable stresses of the respective standards shall be strictly followed while designing the tubes.

(b)Material. - (i)The tubes shall be seamless and manufactured from steel produced by an open hearth or electric process or any of the oxygen processes. The steel shall be fully killed.

(ii)The steel shall conform to the following limits of chemical composition.

Chemical composition (%)
Grade
C
Mn
Si
S
P
TA

0.06-0.18

0.27.-0.63

0.25 max

0.035 max

0.035 max
TB

0.27 max*

0.93 max

0.10 min

0.035 max

0.035 max
TC

0.35 max*

0.29-1.06

0.10 min

0.35 max

0.035 max
* For grade TB and TC for each reduction of 0.01% below the specified carbon maximum, an increase of 0.06% Manganese above the specified maximum will be permitted up to a maximum of 1.35%.

(c)Heat Treatment.- Hot finished tubes need not be heat treated, cold drawn tubes shall be given a sub-critical annealing, a full anneal, or a normalising heat treatment after the final cold finishing process.

(d)Workmanship and Tolerance.-The tubes shall be well finished, cleaned free from harmful defects. They shall be reasonably straight, smooth, cylindrical and subject to the following tolerances. Finished tubes shall be reasonably straight and have smooth ends free of burrs. They shall have a workmanlike finish. Surface imperfections like any discontinuity or irregularity found in the tube may be removed by grinding, provided that smooth curved surface is maintained, and the wall thickness is not decreased to less than that permitted. The outside diameter at the point of grinding may be reduced by the amount so removed.

(i)Permissible variations in outside diameter.
Outside Diameter (mm)
Permissible
variation
Over (mm)
Permissible
variation

Under (mm)
Hot finished seamless tubes

101.6 and under

0.4

0.8
Over 101.6 to 190.5 incl.

0.4

1.2
Over 190.5 to 228.6 incl.

0.4

1.6
Cold finished seamless tubes
Under 25.4

0.1

0.1

25.4 to 38.1 incl.

0.15

0.15
Over 38.1 to 50.8 excl.

0.2

0.2

50.8 to 63.5 excl

0.25

0.25

63.5 to 76.2 excl.

0.3

0.3

76.2 to 101.6 incl.

0.38

0.38
Over 101.6 to 190.5 incl.

0.38

0.64
Over 190.5 to 228.6 incl.

0.38

1.14

3

(ii)Permissible variation in Wall Thickness in percentage.
Outside
diameter

(mm)Wall thickness (mm)

2.4 and under
Over 2.4 to 3.8
Incl.
Over 3.8 to 4.6
incl.
Over 4.6

Over
Under
Over
Under
Over
Under
Over
Under
Seamless Hot Finished tubes

101.6 & under
40
0
35
0
33
0
28
0
Over 101.6
0
0
35
0
33
0
28
0
Seamless Cold Finished tubes

Over
Under

38.1 and under
20
0
Over 38.1

22
0

(iii)Permissible variations in length
Method of manufacture
Outside diameter (mm)
Cut length (mm)
Over
Under
Seamless hot finished
All sizes
5
0
Seamless cold finished
Under 50.8

50.8 and over
3
5
0
0

Note.- These permissible variations in lengths apply to cut lengths up to and including 7.3 m. For lengths over 7.3 m, an additional over tolerance of 3 mm for each 3 m or fraction thereof, shall be permissible, up to a maximum of 13 mm. Length tolerances on the positive side other than specified may be mutually agreed.

37. (a) Test Specimens – (i) Test specimens required for the flattening and expanding/ flaring test specified in regulations 38, 39 and 40 shall be taken from the ends of finished tubes prior to upsetting swaging, expanding or any other forming operations or being cut to length. They shall be smooth on the ends and free from burrs and flaws.

(ii)If desirable and practicable, tensile test may be carried out on full section of the tubes up to the capacity of the testing machine. For large size tubes, the tensile test specimen shall consist of strip cut longitudinally from the tube and which is not straightened within the gauge length and further heat treated.

(iii)If any test specimen shows flaws or defective machining it may be discarded and another specimen substituted.

(iv)All specimens shall be tested at room temperature.

(b)Number of tests. - The test specified in regulations 38, 39 and 40 shall be made on minimum 2 tubes for first 100 tubes and 1 per 100 or part thereof for tubes over 100 numbers.

38. Tensile and Hardness tests. - The test specimen shall comply with the following requirements. The hardness test may be carried out on the wall cross section or on a flat on the outside surface of the tube sample.

4

Grade

Yield
Strength
Mpa
(kg./mm2)
min
Tensile
Strength
Mpa
(kg/mm2)
min
% Elongation
on
GL = 50 mm
min
Hardness
HRB or
HB

Min Max
TA
180(18.3)
325(33.1)
35
77
137
TB
255(26.1)
415(42.2)
30
79
143
TC
275(28.2)
485(49.3)
30
89
179

Note.- For longitudinal strip tests a deduction in percentage elongation 1.5% shall be made for each 0.8 mm decrease in wall thickness under 8mm from the minimum elongation value requirement.

39. Flattening test. -A section of the tube not less than 63 mm in length shall be flattened cold between two parallel flat surfaces to a distance between the plates (H) as calculated by the formula given below, without showing any sign of a crack or flaw.

(1 + e) t 
H =  ----------------- 

E + t/D 

where t   = specified thickness of tube (mm) 

D = specified outside diameter of the tube (mm)
e = a constant, as given below
e = 0.07 for Carbon steel with maximum specified carbon 0.19% or greater e = 0.09 for Carbon steel with maximum specified carbon 0.18% or less

40. Expanding or Flaring test. - A section of the tube approximately 100 mm in length shall stand being flared with a tool having a 60 degree included angle until the tube at the mouth of the flare has been expanded to the percentages given below, without cracking.

Ratio of inside diameter to outside diameter Minimum expansion of inside diameter %

0.9
21

0.8
22

0.7
25

0.6
30
0,5
39

0.4
51

0.3
68

41. Additional test before rejection. - (i) If any one or more tests specified in these regulations fail, two further tests of the same kind may be made on two other tubes of the same batch. If any of these tests fails, the batch of the tubes represented may be given a further heat treatment and entire set of test shall be repeated.

(ii)If the repeat tests are satisfactory the tubes shall be accepted. If any failure in the tests should occur, the entire batch of the tubes shall be rejected.

42. Hydraulic test. - (i) Each tube shall be tested by the manufacturer and shall withstand a hydraulic pressure to one and half times the design pressure subject to a

5
minimum of 1.00 kgf/mm2, but not greater than pressure calculated by the following formula.

2 S t 
P = ------------ 

  D 

where P = test pressure

D = specified outside diameter of the tube t = specified wall thickness of the tube

S = stress which shall be taken as 40% of the minimum tensile strength at room temperature.

(ii)Notwithstanding any thing contained in the above clause, the hydraulic test at the maker’s works may be dispensed with, provided that the tubes are subject to non destructive testing by an appropriate method like Ultrasonic or Eddy Current or Stray Flux testing.

SEAMLESS CARBON STEEL PIPES FOR HIGH TEMPERATURE
SERVICE FOR DESIGN METAL TEMPERATURES NOT EXCEEDING
454 DEGREE C (850 DEGREE F)

43. (a) General - (i) These regulations cover both hot finished and cold drawn seamless carbon steel pipes for high temperature service. The pipes shall conform in all respects with the requirements herein specified.

(ii)The seamless pipes conforming to other national/international standards which are known to be commonly used as being suitable for high temperature service can also be used with the designations of the national/international standards, provided such materials are not specifically prohibited by the regulations.

(iii)While making pipes to other national/internationals standards the allowable stresses of the respective nation/international standards shall be strictly followed while designing the tubes.

(b)Material. - (i) The pipes shall be seamless and manufactured from steel produced by an open hearth or electric process or any of the oxygen processes. The steel shall be fully killed.

(ii)The steel shall conform to the following limits of chemical composition. Grade

Chemical composition %

C

Mn

Si

S
P
PA

0.25*

0.27

0.10

0.035

0.035

Max

0.93 min max max
PB

0.30*

0.29

0.10

0.035

0.035

Min

1.06 min max max
PC

0.35*

0.29

0.10

0.035

0.035

Max

1.06 min max max

6
* For each reduction of 0.01% below the specified carbon maximum, an increase of

0.06% manganese above the specified maximum will be permitted up to a maximum of

1.35%.

(b)Heat treatment. - Hot finished pipes need not be heat treated. Cold drawn pipes shall be given a sub-critical anneal, a full anneal, or a normalising heat treatment after the final cold finishing process.

(c)Workmanship and Tolerance. - The pipes shall be well finished, cleaned free from harmful defects. They shall be reasonably straight, smooth, cylindrical and subject to the following tolerance. Pipes manufacturer shall explore a sufficient number of visual inspections to provide reasonable assurance that they have been properly evaluated.

(i)Permissible variations in outside diameter :

Hot finished and cold finished seamless pipes
Outside diameter

(mm)Permissible variations (mm)
Over Under

10.3 to 48.3 incl.,

0.40

0.79
Over 48.3 to 114.3 incl.,

0.79

0.79
Over 114.3 to 219.1 incl.,

1.59

0.79
Over 219.1 to 457.0 incl.,

2.38

0.79
Over 457.0 to 660.0 incl.,

3.18

0.79
Over 660.0 to 864.0 incl.,

3.97

0.79
Over 864.0 to 1219.0 incl.,

4.76

0.79

(ii)Permissible variation in wall thickness:
The minimum wall thickness at any point shall not be more than 12.5% under the nominal wall thickness specified.

(iii)Permissible variation in exact length:
Seamless Hot finished and Cold finished pipes can be ordered in specified length or in random length. If ordered in specified length, the tolerances for all sizes shall be +6.0 mm/-0.0mm.

(d)Test specimens. - (i) Test specimen required for flattening and expanding/flaring test specified in regulations 44(a), 44(b) and 44(c) shall be taken from ends of finished pipes prior to upsetting, swaging, expanding or any other forming operations or being cut to length. They shall be smooth on ends and free from burrs and flaws.

(ii)If desirable and practicable, tensile test may be carried out on full section of the pipe up to the capacity of the testing machine. For large size pipes, the tensile test specimen shall consist of strip cut longitudinally from the pipe and which is not straightened within the gauge length and further heat treated.

(iii)If any test specimen shows flaws or defective machining it may be discarded and another specimen substituted.

(iv)All specimens shall be tested at room temperature.

7

(e)Number of tests. - The tests specified in regulations 44(a), 44(b) and 44(c) shall be made on minimum 2 pipes for first 100 pipes and 1 per 100 or part thereof for pipes over 100 numbers.

44. (a) Tensile test. - Test pieces cut from the ends of the selected pipes shall comply with the following requirements. The tensile test may be carried out on the test pieces cut out from the pipe in the longitudinal direction which shall not be further heat treated nor straightened within the gauge length. As an alternative, pipes may be tested on full cross section.

Grade
Yield Strength
MPa (kg/mm2)
min
Tensile Strength
Mpa (kg/mm2)
Min
%Elongation
on G.L.=50mm
min
PA
205 (21.1)
330(33.1)
35
PB
240 (24.7)
415 (42.2)
30
PC
275 (28.2)
485 (49.3)
30

For longitudinal strip test, the minimum required elongation shall be determined by the following equation.

e = 1942.57 (A 0.02/U0.9)

where e = minimum elongation in 50.8 mm, % rounded to the nearest 0.5%. A = cross sectional area of the tensile test specimen in mm2 based on specified outside diameter or nominal specimen width and specified wall thickness rounded to the nearest 6.45 mm2. If the area thus calculated is more than 484 mm2 then use area as 484 mm2. If the calculated area is less than 484mm2 then use the actual area thus obtained.

U = specified tensile strength in Mpa.

(b)Bend test. - For pipes of outside diameter 60.3 mm and under, a bend test shall be conducted. A sufficient length of pipe shall stand being bent cold through 90 degree around a cylindrical mandrel, the diameter of which is 12 times the nominal diameter of the pipe, without developing cracks.

(c)Flattening test. - (i) For pipes of outside diameter over 60.3 mm, a flattening test shall be conducted. A section of the pipe not less than 63 mm in length shall be flattened cold between two parallel flat surfaces to a distance between the plates (H) as calculated by the formula given below, without showing any sign of a crack or flaw.

         (1 + e) t 
H =  ----------- 
         e + t/D 

where t = specified thickness of pipe (mm)

D = specified outside diameter of the pipe (mm)

e = a constant, as given below e = 0.07 for carbon steel with maximum specified carbon 0.19% or more e = 0.09 for carbon steel with maximum specified carbon 0.18% or less.

8

(ii)For pipe whose diameter equals or exceeds 254 mm, a bend test may be conducted instead of the flattening test. The bend test specimens shall be bent at room temperature through 180 degree without cracking on the outside of the bent portion. The inside diameter of the bend shall be 25 mm. Substitution of the bend test for the flattening test shall be subject to the approval of the purchaser.

(iii)For pipe whose diameter exceeds 635 mm and whose diameter to wall thickness ratio is 7.0 or less, the bend test described in clause (b) shall be conducted instead of the flattening test.

45. Additional tests before rejection. - If any one or more tests specified in these regulations fail, two further tests of the same kind may be made on two other pipes of the same batch. If any of these tests fails, the batch of the pipes represented may be given a further heat treatment and entire set of tests shall be repeated.

If the repeat tests are satisfactory the pipes shall be accepted. If any failure in the tests should occur the entire batch of the pipes shall be rejected.

46. Hydraulic test. - (i) Each pipe shall be tested by the manufacturer and shall withstand a hydraulic pressure to one and half time the design pressure, but not greater than pressure calculated by the formula given below. In the absence of working pressure indicated in the Test Certificate then the test pressure indicated in the Test Certificate divided by 1.5 shall be the maximum working pressure.

P = 2St/D where P = test pressure

D = specified outside diameter of the pipe t = specified wall thickness of the pipe
S = stress which shall be taken as 40% of the minimum tensile strength at room temperature.

(ii)Notwithstanding anything contained in the above clause, the hydraulic test at the maker's works may be dispensed with provided that the pipes are subject to non destructive testing by an appropriate method like Ultrasonic or Eddy Current or Stray flux testing.

SEAMLESS FERRITIC AND AUSTENITIC ALLOY STEEL
BOILER, SUPERHEATER AND HEAT EXCHANGER TUBES

47. General. - (i) These regulations cover both hot finished and cold drawn seamless boiler, superheater and heat exchanger tubes of ferritic and austenitic alloy steel grades. These shall conform in all respects with the requirements herein specified.

(ii)The seamless tubes conforming to other national/international standards which are known to be commonly used as being suitable for use as boiler and superheater tubes can also be used with the designations of the national/international standards, provided such materials are not specifically prohibited by the regulations.

9

(iii)While making tubes to other national/internationals standards the allowable stresses of the respective standard shall be strictly followed while designing the tubes.

(iv)The design metal temperatures shall not exceed the following limits :-

Grade

Temp.

Degree C(Degree F)

T1, T2

537 (1000)

T5, T9, T11, T12, T22, T91, 12X1Mo, X20CrMoV121,
TP 304, TP 304H, TP 304L, TP 310S, TP 316, TP316H,
TP 316L, TP321, TP321H, TP347, TP347H

648 (1200)

48. (a) Material. - (i) The tubes shall be seamless and manufactured from steel produced by an open hearth or electric process or any of the oxygen processes. The steel shall be fully killed.

(ii)The steel shall conform to the limits of chemical compositions given in Table-1 and 2.

(iii)The grain size of cold worked grade TP 321H shall be No.7 or coarser.

(b)Heat treatment. - (i) All tubes of grades in Table-1, except T 91, 12X1Mo and X20CrMoV121 shall be reheated and furnished in full annealed, isothermal annealed or normalised and tempered condition. If furnished in the normalised and tempered condition, the minimum tempering temperature for Grades T1 and T11 shall be 650 degree C and the minimum tempering temperature for Grades T5, T9 and T22 shall be 675 Degree C.

(ii)Tubing of Grades T1, T2 and T12 either hot finished or cold drawn, may be given a final heat treatment at 650 degree C to 730 degree C, instead of heat treatments specified in sub-clause (i) above, at the option of the manufacture.

(iii)Grade T91 shall be normalised at 1040 degree C minimum and tempered at 730 degree C minimum as a final heat treatment.

(iv)Grade 12x1Mo shall be normalised at 950 - 980 degree C and tempered at 720 - 750 degree C for a period of 1 to 3 hours.

(v)Grade X20CrMoV121 shall be normalised at 1020 - 1070 degree C and tempered at 730 - 780 degree C for a period of 1 hour minimum.

(vi)All austenitic tubes (Table 2) shall be furnished in the heat treated condition. The heat treatment procedure, except for the H grades shall consist of heating the material to a minimum temperature of 1040 degree C and quenching in water or rapidly cooling by other means.

(vii)All H grades shall be furnished in the solution treated condition. If cold working is involved in processing, the minimum solution treating temperatures for grades TP321H and TP347H shall be 1100 degree C and for grades TP304H and TP316H shall be 1040

10
degree C. If the P grade is hot rolled, the minimum solution treatment for grades TP 321 H and TP 347 H shall be 1050 degree C and for grades TP 304H and TP 316H shall be 1040 degree C.

(c)Workmanship and tolerance - The tubes shall be well finished, cleaned free from harmful defects. They shall be reasonably straight, smooth, cylindrical and subject to the following tolerances. Finished tubes shall be reasonably straight and have smooth ends free of burrs. They shall have a workmanlike finish. Surface imperfections like any discontinuity or irregularity found in the tube may be removed by grinding, provided that a smooth curved surface is maintained, and the wall thickness is not decreased to less than that permitted. The outside diameter at the point of grinding may be reduced by the amount so removed.

(i)Permissible variation in outside diameter:

For all grades except 12X1Mo and X20CrMoV121
Outside diameter (mm)
Permissible Variation (mm)
Over
Under
Hot finished Seamless tubes

101.6 and under

0.4

0.8
Over 101.6 to 190.5 incl.

0.4

1.2
Over 190.5 to 228.6 incl.

0.4

1.6
Cold finished Seamless tubes
Under 25.4

0.10

0.10
Over 25.4 to 38.1 incl.

0.15

0.15
Over 38.1 to 50.8 excl.

0.20

0.20

50.8 to 63.5 excl.

0.25

0.25

63.5 to 76.2 excl.

0.30

0.30

76.2 to 101.6 incl.

0.38

0.38
Over 101.6 to 190.5 incl.

0.38

0.64
Over 190.5 to 228.6 incl.

0.38

1.14

For grade 12X1Mo
Outside diameter (mm)
Permissible Variation (mm)
Over
Under
Hot finished and cold finished tubes
Under 30.0

0.30

0.30
30 to 50

0.40

0.40
Over 50.0

0.80%

0.80%

For grade X20CrMoV121
Outside diameter
Permissible Variation (mm)
Over
Under
Hot finished Seamless tubes
100 and under

0.75% (0.5 mm min)

0.75% (0.5 mm min)
Cold finished seamless tubes
120 and under

0.60% (0.25 mm min)

0.60%(0.25 mm min)
Over 120

0.75%

0.75%

11

(ii)Permissible variation in Wall Thickness :

For all grades except 12X1Mo and X20CrMoV121
Outside
Diameter

(mm)

Wall thickness %

2.4 and under
Over 2.4 to 3.8
incl.
Over 3.8 to 4.6
incl.
Over 4.6

Over
Under
Over
Under
Over
Under
Over
Under
Seamless hot finished tubes

101.6
and
Under
40
0
35
0
33
0
28
0
Over 101.6
0
0
35
0
33
0
28
0
Seamless cold finished tubes

Over
Under

38.1 and under
20
0
Over 38.1
22
0

For Grade 12X1Mo
Outside Diameter (mm)
Permissible variation %
Over
Under
Hot Finished Seamless Tubes
108 and under
15
10
Over 108
20
5
Cold Finished Seamless Tubes
All sizes
10
10

For Grade X20CrMoV121
Outside diameter (mm)
Permissible variation %
Over
Under
100 and under

12.5
10

(iii)Permissible variation in length for exact length tubes.

For all Grades except 12 X 1Mo and X20CrMoV121
Method of manufacture
Outside diameter (mm)
Cut length (mm)
Over Under
Seamless Hot finished
All sizes

50
Seamless Cold finished
Under 50.8
30

Columns reconstructed from the extracted text; check against the Gazette page.

Show original extracted text (diagnostic, not authoritative)
   5                             0 
Seamless Cold finished 
Under 50.8 
   3                             0 

50.8 Over

5                             0 

Note : These permissible variations in lengths apply to cut lengths upto and including 7.3 m. For lengths over 7.3 m, an additional over tolerance of 3 mm for each 3 m or fraction thereof, shall be permissible, upto a maximum of 12 mm.

12

For grade 12X1Mo
Out side diameter (mm)
Length of tubes (m)
Permissible variation (mm)
Over Under
Under 108
Under 9

150
9 to12
35
0
108and over
Alllengths
50
0

Columns reconstructed from the extracted text; check against the Gazette page.

Show original extracted text (diagnostic, not authoritative)
      15                         0 
9 to 12 
      35                         0 
108 and over 
All lengths 
      50                         0 

For grade X20CrMoV121
Length of tube (m)
Permissible variation (mm)
Over Under
6 and under
10
0
Over 6 to 12 incl.
15
0

(d)Test specimens. - (i) Test specimens required for the flattening and expanding/ flaring test specified in regulations 49(a), 49 (b) and 49(c) shall be taken from the ends of finished tubes prior to upsetting, swaging, expanding or any other forming operations or being cut to length. They shall be smooth on the ends and free from burrs and flaws.

(ii)If desirable and practicable, tensile test may be carried out on full section of the tubes upto the capacity of the testing machine. For large size tubes, the tensile test specimen shall consist of strip cut longitudinally from the tube and which is not straightened within the gauge length further heat treated.

(iii)If any test specimen shows flaws or defective machining it may be discarded and another specimen substituted.

(iv)All specimens shall be tested at room temperature.

(e)Number of tests. - The tests specified in regulations 49(a), 49(b) and 49(c) shall be made on minimum 2 tubes for first 100 and 1 per 100 or part thereof for tubes over 100 numbers.

49. (a) Tensile and hardness tests. - The test specimen shall comply with the requirements as given in Table 3. The hardness test may be carried out on the wall cross section or on a flat on the outside surface of the tube sample.

(b)Flattening test. - A section of the tube not less than 63 mm in length shall be flattened cold between two parallel flat surfaces to a distance between the plates (H) as calculated by the formula given below, without showing any sign of a crack of flaw.

(1 + e)t 

    H = ----------- 
             e + t/D 

where t = specified thickness of tube (mm)

D = specified outside diameter of the tube (mm)

e = a constant, as given below e = 0.08 for ferritic alloy steel e = 0.09 for austenitic steel

13

(c)Expanding or flaring test. - A section of the tube approximately 100 mm in length shall stand being flared with a tool having a 60 degree included angle until the tube at the mouth of the flare has been expanded to the percentages given below, without cracking.

Ratio of inside diameter to outside diameter
Minimum expansion of inside diameter %

0.9
21

0.8
22

0.7
25

0.6
30

0.5
39

0.4
51

0.3
68

50. Additional tests before rejection. - (i) If any one or more tests specified in these regulations fail, two further tests of the same kind may be made on two other tubes of the same batch. If any of these tests fails, the batch of the tubes represented may be given a further heat treatment and entire set of tests shall be repeated.

(ii)If the repeat tests are satisfactory the tubes shall be accepted. If any failure in the tests should occur the entire batch of the tubes shall be rejected.

51. Hydraulic test. - (i) Each tube shall be tested by the manufacturer and shall withstand a hydraulic pressure to one and a half time the design pressure subject to a minimum of 1.00 kgf/mm2, but not greater than pressure calculated by the following formula:-

P = 2 St/D where P = test Pressure
D = specified out side diameter of the tube t = specified wall thickness of the tube

S = stress which shall be taken as 40% of the minimum tensile strength at room temperature.

(ii)Notwithstanding anything contained in the above clause, the hydraulic test at the maker's works may be dispensed with, provided that the tubes are subject to non destructive testing by an appropriate method like Ultrasonic or Eddy current or Stray Flux testing.

14

TABLE 1
CHEMICAL REQUIREMENTS FOR FERRITIC STEELS
Grade
Chemical composition %

C
Mn
Si
S
P
Cr
Mo
V
Ni
Other
Elements
T1

0.10

0.20

0.30

0.80

0.10

0.50

0.025
max

0.025

max 

------- 0.44 
0.65 

---
---
----
T2

0.10

0.20

0.30

0.61

0.10

0.30

0.025
max

0.025
max

0.50

0.81

0.44

0.65
----

--- 
----- 
T5 

0.15
max

0.30

0.60

0.50
max

0.025
max

0.025
max

4.00

6.00

0.45

0.65
----

---- 
----- 
T9 

0.15
max

0.30

0.60

0.25

1.00

0.025
max

0.025
max

8.00

10.0

0.90

1.10
----

---- 
----- 
T11 

0.05

0.15

0.30

0.60

0.50

1.00

0.025
max

0.025
max

1.00

1.50

0.44

0.65
----

---- 
----- 
T12 

0.05

0.15

0.30

0.61

0.50
max

0.025
max

0.025
max

0.80

1.25

0.44

0.65
----

--- 
          ----- 
T22 

0.05

0.15

0.30

0.60

0.50
max

0.025
max

0.025
max

1.90

2.60

0.87

1.13
----

---- 
          ----- 
T91 

0.08

0.12

0.30

0.60

0.20

0.50

0.010
max

0.020
max

8.00

9.50

0.85

1.05

0.18

0.25
----
Nb=0.06 - 0.10
N=0.030 - 0.70
Ni=0.40 max
Al=0.04 max
12X1
Mo

0.10

0.15

0.40

0.70

0.17

0.37

0.025
max

0.025
max

0.90

1.20

0.25

0.35

0.15

0.30

0.25
max
Cu=0.20
Max
X20
CrMoV
121

0.17

0.23

1.00
max

0.50
max

0.030
max

0.03
max

10.0

12.5

0.80

1.20

0.25

0.35

0.30

0.80

TABLE 2
CHEMICAL REQUIREMENTS OF AUSTENTIC STEEL
Grade
Chemical composition %

C
Mn
Si
S
P
Cr
Mo
V
Ni
Other
Elements
TP304

0.08
max

2.00
max

0.75
max

0.030
max

0.40
max

18.0

20.0
----
----

8.00

11.0
----
TP304H 0.04

0.10

2.00
max

0.75
max

0.030
max

0.040
max

18.0

20.0 
----- 
---- 

8.00

11.0 
----- 
TP304L 

0.035
max

2.00
max

0.75
max

0.030
max

0.040
max

18.0

20.0 
----- 
---- 

8.00

13.0 
----- 
TP310S 

0.08
max

2.00
max

0.75
max

0.030
max

0.045
max

24.0

26.0

0.75
max
----

19.0

22.0 
----- 
TP316 

0.08
max

2.00
max

0.75
max

0.030
max

0.040
max

16.0

18.0

2.00

3.00
----

11.0

14.0 
----- 
TP316H 0.040 

0.10

0.10

2.00
max

0.75
max

0.030
max

0.040
max

16.0

18.0

2.00

3.00
----

11.0

14.0 
----- 


15

TP316L

0.035
max

2.00
max

0.75
max

0.030
max

0.040
max

16.0

18.0

2.00

3.00
----

10.0

15.0 
----- 
TP321 

0.08
max

2.00
max

0.75
max

0.030
max

0.040
max

17.0

20.0
----
----

9.00

13.0
Ti=5xC min

0.60 max
TP321H 0.04

0.10

2.00
max

0.75
max

0.030
max

0.040
max

17.0

20.0
----
----

9.00

13.0
Ti=4xC min

0.60 max
TP347

0.08
max

2.00
max

0.75
max

0.030
max

0.040
max

17.0

20.0
----
----

9.00

13.0
Nb+Ta=10xC
min

1.000 max
TP347H 0.04

0.10

2.00
max

0.75
max

0.030
max

0.040
max

17.0

20.0

---- 
----- 
9.00 

13.00
Nb+Ta=8xC
min

1.00 max

TABLE 3
MECHANICAL PROPERTY REQUIREMENTS
Grade
Yield strength
Mpa (kg/mm2)
Min
Tensile Strength
Mpa (kg/mm2)
Min
%
Elongation
on
GL=50mm
min *
Hardness

HRB HB
max max
T1
205 (21.1)
380 (38.7)
30

80                 146 

T2
205 (21.1)
415 (42.2)
30

85                 163 

T5
205 (21.1)
415 (42.2)
30

85                  163  

T9
205 (21.1)
415 (42.2)
30

89                 179 

T11
205 (21.1)
415 (42.2)
30

85                 163 

T12
220 (22.5)
415 (42.2)
30

85                 163 

T22
205 (21.1)
415 (42.2)
30

85                 163 

T91
415 (42.2)
585 (59.6)
20

25 HRC        250    

12X1Mo
274 (28.0)
441 (45.0)
637 (65.0)
21

85                 163 

X20Cr
MoV121
490 (50.0)
690 (70.4)
840 (85.7)
17

25HRC        250 

TP 304
205 (21.1)
515 (52.5)
35

90                 192 

TP304H
205 (21.1)
515 (52.5)
35

90                 192 

TP304L
170 (17.3)
485 (49.5)
35

90                 192 

TP310S
205 (21.1)
515 (52.5)
35

90                 192 

TP316
205 (21.1)
515 (52.5)
35

90                 192 

TP316H
205 (21.1)
515 (52.5)
35

90                 192 

TP316L
170 (17.3)
485 (49.5)
35

90                 192 

TP321
205 (21.1)
515 (52.5)
35

90                 192 

TP321H
205 (21.1)
515 (52.5)
35

90                 192 

TP347
205 (21.1)
515 (52.5)
35

90                 192 

TP347H
205 (21.1)
515 (52.5)
35

90                 192 

*GL = 5.65SO

16
SEAMLESS FERRITIC PIPES FOR HIGH TEMPERATURE SERVICE

52. General. - (i)These regulations cover both hot finished and cold drawn seamless pipes of ferritic alloy steel grades. These shall conform in all respects with the requirements herein specified.

(ii)The seamless pipes conforming to other national/international standards which are known to be commonly used as being suitable for high temperature service can also be used with the designations of the national/international standards, provided such materials are not specifically prohibited by the regulations.

(iii)While making pipes to other national/international standards the allowable stresses of the respective standard shall be strictly followed while designing the tubes.

(iv)The design metal temperatures shall not exceed the following limits Grade

Temp. Degree C (Degree F)

P1, P2

537 (1000)

P5, P9, P11, P12, P22, P91, X20CrMoV121
648 (1200)

53. (a). Material. - (i) The pipes shall be seamless and manufactured from steel produced by an open hearth or electric process or any of the Oxygen processes. The steel shall be fully killed.

(ii)The steel shall conform to the limits of chemical composition as given in table-4.

(b)Heat treatment. - (i) All pipes of grades in table-1 except P91 and X20CrMoV121 shall be reheated and furnished in full annealed, isothermal annealed or normalised and tempered condition. If furnished in the normalised and tempered condition, the minimum tempering temperature for grade P1, P2, P11 and P12 shall be 650 degree C and the minimum tempering temperature for grades P5, P9 and P22 shall be 675 degree C.

(ii)Pipes of grades P1, P2 and P12 either hot finished or cold drawn may be given a final heat treatment at 650 degree C to 705 degree C, instead of heat treatment specified in sub-clause (i) above at the option of the manufacturer.

(iii)Grades P91 shall be normalised at 1040 degree C minimum and tempered at 730 degree minimum as a final heat treatment.

(iv)Grades X20CrMoV121 shall be normalised at 1020 - 1070 degree C and tempered at 730-780 degree C for a period of one hour minimum.

(c)Workmanship and tolerance - The pipes shall be well finished, cleaned free from harmful defects. They shall be reasonably straight, smooth, cylindrical and subject to the following tolerances. Pipes manufacturer shall explore a sufficient number of visual inspections to provide reasonable assurance that they have been properly evaluated.

17

(i)Permissible variation in outside diameter.

For all grades except X20CrMoV121
Hot finished and Cold finished seamless pipes

Outside diameter                                                     Permissible variations (mm) 
(mm)                                                                       Over                                 Under 

10.3 to 48.3 incl.

0.40

0.79
Over 48.3 to 114.3 incl.

0.79

0.79
Over 114.3 to 219.1 incl.

1.58

0.79
Over 219.1 to 457.0 incl.

2.38

0.79
Over 457.0 to 660.0 incl.

3.18

0.79
Over 660.0 to 864.0 incl.

3.97

0.79
Over 864.0 to 1219.0 incl.

4.76

0.79

For Grade X20CrMoV121
Over 100 to 320 incl.

0.90%

0.90%
Over 320

1.00%

1.00%

(ii)Permissible variations in wall thickness :
For all grades, except X20CrMoV121
The minimum wall thickness at any point shall not be more than 12.5% under the nominal wall thickness specified.

For grade X20CrMoV121
Outside diameter (mm)
Permissible variation %
Over Under
Over 100 to 320 incl.

12.5

12.5
Over 320

15.0

12.5

(iii)Permissible variation in length :
Seamless Hot finished and Cold finished pipes can be ordered in specified length or in random length. If ordered in specified length, the tolerance shall be as follows :

For hot finished and cold finished pipes
Grade
Length (m)
Permissible variation in (mm)
Over Under
All grades except
X20CrMoV121
All length

6                               0 

For grade
X20CrMoV121
6 and under
Over 6 to 12 incl.

10                              0 
   15                               0 

(d)Test specimen - (i) Test specimens required for flattening and expanding/flaring test specified in regulations 54(a), 54(b) and 54(c) shall be taken from ends of finished pipes prior to upsetting, swaging, expanding or any other forming operations or being cut to length. They shall be smooth on ends and free from burrs and flaws.

18

(ii)If desirable and practicable, tensile test may be carried out on full section of the pipe upto the capacity of the testing machine. For large size pipes the tensile test specimen shall consist of strip cut longitudinally from the pipe and which is not straightened within the gauge length and further heat treated.

(iii)If any test specimen shows flaws or defective machining it may be discarded and another specimen substituted.

(iv)All specimens shall be tested at room temperature.

(e)Number of tests - (i) The tests specified in regulations 54(a), 54(b) and 54(c) shall be made on minimum 2 pipes for first 100 pipes and 1 per 100 part thereof for pipes over 100 numbers.

54. (a)Tensile test. - The test specimen shall comply with the requirements given in the table 5.

(b)Bend test. - For pipes of outside diameter 60.3 mm and under, a bend test shall be conducted. A sufficient length of pipe shall stand being bent cold through 90 around a cylindrical mandrel, the diameter of which is 12 times the nominal diameter of the pipe, without developing cracks.

(c)Flattening test. - (i) For pipes of outside diameter over 60.3 mm a flattening test shall be conducted. A section of the pipe not less than 63 mm is length shall be flattened cold between two parallel flat surfaces to a distance between the plates (H) as calculated by the formula given below, without showing any sign of a crack or flaw.

H = (1+e) t / {e + (t/D)} where t = specified thickness for pipe (mm)
D = specified outside diameter of the pipe (mm)
e = a constant, 0.08 for ferritic alloy steel.

(ii)For pipe whose diameter equals or exceeds 254 mm, a bend test may be conducted instead of the flattening test. The bend test specimens shall be bent at room temperature through 180 degree C without cracking on the outside of the bent portion. The inside diameter of the bend shall be 25 mm. Substitution of the bend test for the flattening test shall be subject to the approval of the purchaser.

(iii)For pipes whose diameter exceed 635 mm and whose diameter to wall thickness ratio is 7.0 or less, the bend test described in clause (b) shall be conducted instead of the flattening test.

55. Additional tests before rejection. - (i) If any one or more tests specified in these regulations fail, two further tests of the same kind may be made on two other pipes of the same batch. If any of these tests fails, the batch of the pipes represented may be given a further heat treatment and entire set of tests shall be repeated.

(ii)If the repeat tests are satisfactory, the pipes shall be accepted. If any failure in the tests should occur the entire batch of the pipes shall be rejected.

19

56. Hydraulic test. - (i) Each pipe shall be tested by the manufacturer and shall withstand a hydraulic pressure to one and half times the design pressure but not greater than pressure calculated by the following formula given below. In the absence of working pressure is indicated in the Test Certificate then the tested pressure indicated in the Test Certificate divided by 1.5 shall be the maximum working pressure

P = 2 S t / d where P = test pressure

D = specified outside diameter of the pipe t = specified wall thickness of the pipe
S = stress which shall be taken as 40% of the minimum tensile strength at room temperature.

(ii)Notwithstanding anything contained in the above clause, the hydraulic test at the maker's works may be dispensed with provided that the pipes are subject to non destructive testing by an appropriate method like Ultrasonic or Eddy current or stray flux testing

Table 4
CHEMICAL REQUIREMENTS FOR FERRITIC STEELS
Grade
Chemical composition %

C

Mn

Si

S

P

Cr

Mo

V

Ni
Other
Elements

P1

0.10

0.20

0.30

0.80

0.10

0.50

0.025
max

0.025
max

----

0.44

0.65

----

---- 
----- 
P2 

0.10

0.20

0.30

0.61

0.10

0.30

0.025
max

0.025
max

0.50

0.81

0.44

0.65
----

---- 
----- 
P5 

0.15
max

0.30

0.60

0.50
max

0.025
max

0.025
max

4.00

6.00
o.45

0.65
----

---- 
----- 
P9 

0.15
max

0.30

0.60

0.25

1.00

0.025
max

0.025
max

8.00

10.0

0.90

1.10
----

---- 
----- 
P11 

0.05

0.15

0.30

0.60

0.50

1.00

0.025
max

0.025
max

1.00

1.50

0.44

0.65
----

---- 
----- 
P12 

0.05

0.15

0.30

0.61

0.50
max

0.025
max

0.025
max

0.80

1.25

0.44

0.65
----

---- 
----- 
P22 

0.05

0.15

0.30

0.60

0.50
max

0.025
max

0.025
max

1.90

2.60

0.87

1.13
----

---- 
----- 
P91 

0.08

0.12

0.30

0.60

0.20

0.50

0.010
max

0.020
max

8.00

9.50

0.85

1.05

0.18

0.25
----
Nb=0.06 - 0.10
N=0.030 - 0.70
Ni=0.40 max
Al=0.04 max
X20Cr
MoV121

0.17

0.23

1.00
max

0.50
max

0.03
max

0.030
max

10.0

12.5

0.80

1.20

0.25

0.35

0.30

0.80
----

20

Table-5
MECHANICAL PROPERTY REQUIREMENTS
Grade

Yield Strength Mpa
(kg/mm2) min
Tensile Strength
Mpa (kg/mm2) min
% elongation on
GL=50mm min *
P1
205(21.1)
380(38.7)
30
P2
205(21.1)
380(38.7)
30
P5
205(21.1)
415(42.2)
30
P9
205(21.1)
415(42.2)
30
P11
205(21.1)
415(42.2)
30
P12
220(22.5)
415(42.2)
30
P22
205(21.1)
415(42.2)
30
P91
415(42.2)
585(59.8)
20
X20CrMoV121
490(50.0)
690(70.4)
840(85.6)
17

*GL=5.65SO.".

[File No. 6(11)/2000-Boilers]

Sd/-
(V.K. GOEL)
Secretary, Central Boilers Board

Foot note.- The principal regulations were published in the Gazette of India vide S.O. 600, dated the 15th September, 1950 and subsequently amended vide notifications –

(i)

G.S.R. 178, dated the 24th March, 1990;

(ii)

G.S.R. 179, dated the 24th March, 1990;

(iii)

G.S.R. 488, dated the 9th October, 1993;

(iv)G.S.R. 516 dated the 23rd October, 1993;

(v)G.S.R. 634 dated the 25th December, 1993;

(vi)G.S.R. 107 dated the 26th February, 1994;
Errata G.S.R. 223 dated the 14th May, 1994;

(vii)G.S.R. 250 dated the 4th June, 1994;

(viii)G.S.R. 402 dated the13th August, 1994;

(ix)

G.S.R. 427 dated the 20th August, 1994;

(x)

G.S.R. 562 dated the12th November, 1994;

(xi)

G.S.R. 607 dated the10th December, 1994;

(xii)

G.S.R. 83 dated the 25th February, 1995;

(xiii)G.S.R. 93 dated the 4th March, 1995;

(xiv)G.S.R. 488 dated the 9th November, 1996;

(xv)

G.S.R. 582 dated the 28th December, 1996;

(xvi)G.S.R. 59 dated the 25th January, 1997;

(xvii)G.S.R. 117 dated the 1st March, 1997;

(xviii)G.S.R. 172 dated the 29th March, 1997.

(xix)G.S.R. 221 dated the 21st November, 1998.

21

(xx)

G.S.R. 131 dated 1st May, 1999.

(xxi)G.S.R. 139 dated 8th May, 1999.

(xxii)G.S.R. 237 dated 31st July, 1999.

(xxiii)G.S.R. 345 dated 23rd October, 1999.

(xxiv)G.S.R. 397 dated 14th October, 2000.

To

The General Manager,

Government of India Press,

Ring Road, Mayapuri,

New Delhi-110064.